Ir-doped Co3O4 nanocatalysts, their preparation methods and applications, and metal-air batteries
By adjusting the electronic structure of Ir-doped Co3O4 nanocatalysts, the kinetic problems of OER and ORR reactions in metal-air batteries were solved, achieving efficient and low-cost bifunctional catalysis and improving the energy density and cycle life of the battery.
Patent Information
- Application Number
- CN202311709832.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-13
AI Technical Summary
Existing metal-air batteries suffer from slow reaction kinetics and high overpotentials during charging and discharging of the OER and ORR reactions, which limit their energy efficiency and cycle life. Furthermore, existing precious metal catalysts are expensive, scarce, and have poor durability.
Ir-doped Co3O4 nanocatalysts were used, incorporating Ir into Co3O4 via impregnation to adjust the electronic structure, increase active sites, and lower the reaction energy barrier, thereby achieving bifunctional catalysis.
Ir-doped Co3O4 nanocatalysts exhibit excellent catalytic activity in OER and ORR processes, reducing catalyst costs and improving the energy density and cycle stability of metal-air batteries.
Smart Images

Figure CN117673383B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical technology, and in particular to an Ir-doped Co3O4 nanocatalyst, its preparation method and application, and metal-air batteries. Background Technology
[0002] Metal-air batteries possess significant advantages such as high energy density, safety, low cost, and environmental friendliness, showing great potential in portable flexible electronic devices. However, the OER and ORR reactions occurring at the cathode during charging and discharging in metal-air batteries involve four-electron multi-step processes, resulting in slow reaction kinetics and high overpotentials. These limitations severely restrict the energy efficiency and cycle life of metal-air batteries, hindering their practical application.
[0003] Currently, the most active monofunctional catalysts for OER and ORR are RuO2 and Pt / C, respectively, both noble metal-based materials. However, their high cost, scarcity, and poor durability limit their large-scale application. Furthermore, while combining two monofunctional catalysts can achieve bifunctional catalysis, this combination further increases the cost and complexity of fabrication. Therefore, there is an urgent need to develop efficient and low-cost bifunctional catalysts for OER and ORR.
[0004] In view of this, the present invention is hereby proposed. Summary of the Invention
[0005] One of the objectives of this invention is to provide a method for preparing Ir-doped Co3O4 nanocatalysts to solve at least one of the aforementioned technical problems.
[0006] The second objective of this invention is to provide an Ir-doped Co3O4 nanocatalyst.
[0007] The third objective of this invention is to provide an application of Ir-doped Co3O4 nanocatalyst in catalytic electrochemical reactions.
[0008] The fourth objective of this invention is to provide a metal-air battery.
[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0010] The first aspect of this invention provides a method for preparing Ir-doped Co3O4 nanocatalysts, comprising the following steps:
[0011] A. Add an iridium-containing compound solution dropwise to a Co3O4 dispersion at a rate ≤60 μL / min to obtain a mixed solution; after the mixed solution is dried for the first time, a semi-finished Ir-doped Co3O4 nanocatalyst is obtained.
[0012] B. The Ir-doped Co3O4 nanocatalyst semi-finished product is placed in a tube furnace and annealed at 200℃~300℃. After washing and second drying, the Ir-doped Co3O4 nanocatalyst is obtained.
[0013] Furthermore, the iridium-containing compound includes chloroiridium acid and / or iridium chloride.
[0014] Preferably, the solvent in the iridium-containing compound solution includes water.
[0015] Preferably, the concentration of the iridium-containing compound solution is 10 mg / mL to 40 mg / mL.
[0016] Furthermore, the dispersant of the Co3O4 dispersion includes an alcohol.
[0017] Preferably, the alcohol includes at least one selected from methanol, ethanol, isopropanol, and n-propanol.
[0018] Preferably, the concentration of the Co3O4 dispersion is 1 mg / mL to 3 mg / mL.
[0019] Further, in step A, the mass ratio of the iridium-containing compound to Co3O4 is 0.1 to 1:1, preferably 0.1 to 0.5:1.
[0020] Furthermore, the temperature of the first drying process is 60℃~90℃, and the time is 8h~16h.
[0021] Furthermore, in step B, the heating rate is 5°C / min to 10°C / min.
[0022] Preferably, the annealing time is 1 hour to 4 hours.
[0023] Preferably, the washing is performed 3 to 6 times using deionized water.
[0024] Preferably, the second drying is carried out in a vacuum oven, the temperature of which is set to 80℃~120℃ and the time to be 8h~24h.
[0025] The second aspect of the present invention provides an Ir-doped Co3O4 nanocatalyst prepared by the preparation method described above.
[0026] The third aspect of this invention provides the application of the Ir-doped Co3O4 nanocatalyst in catalytic electrochemical reactions.
[0027] Furthermore, the electrochemical reactions include the oxygen evolution reaction (OER) and the oxygen reduction reaction (ORR).
[0028] A fourth aspect of the present invention provides a metal-air battery, comprising an air electrode, a metal electrode, and an electrolyte solution;
[0029] The metal electrode may contain magnesium, aluminum, zinc, mercury or iron.
[0030] A catalyst layer is disposed on the air electrode, and the catalyst in the catalyst layer is the Ir-doped Co3O4 nanocatalyst.
[0031] Compared with the prior art, the present invention has at least the following beneficial effects:
[0032] The preparation method provided by this invention uses spinel oxide Co3O4 as a base material. Co3O4 possesses multiple metal valences, controllable composition, and tunable morphology, playing a crucial role in electron transfer and metal redox cycles. Ir is incorporated into Co3O4 via an impregnation method, increasing the number of active sites in the material. Due to the different electronegativity of Ir and Co, Ir doping induces electron transfer between Ir and Co, adjusting the valence state and electronic structure of Co, thereby modifying the resistance to OH in the OER and ORR processes. - The adsorption and desorption capabilities of the catalyst enhance the reaction energy barrier and improve the catalytic performance of OER and ORR. This preparation method is simple, energy-efficient, and environmentally friendly, improving atom utilization and achieving low loading and high catalytic performance.
[0033] The Ir-doped Co3O4 nanocatalyst provided by this invention incorporates Ir into the Co3O4 lattice, thereby regulating the electronic structure, improving conductivity, and increasing active sites, thus achieving bifunctional catalysis. The ORR half-wave potential of this Ir-doped Co3O4 nanocatalyst is 0.81 V; 10 mA / cm². 2 The OER potential at the current density is 1.488V, and the difference between the two potentials is only 0.678V, which shows excellent bifunctional catalytic activity.
[0034] The application of Ir-doped Co3O4 nanocatalysts provided by this invention in catalytic electrochemical reactions offers a catalyst with better performance and multiple functions, reduces the cost of catalyst use, and expands the development of downstream industries.
[0035] The metal-air battery provided by this invention has a peak power density of 195 mW / cm³. 2 It also exhibits a cycle stability of up to 1200 hours, making large-scale application of metal-air batteries possible. Attached Figure Description
[0036] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0037] Figure 1 Here is a high-magnification transmission electron microscopy image of the Ir-doped Co3O4 nanocatalyst obtained in Example 2;
[0038] Figure 2 The elemental distribution characterization diagram of the Ir-doped Co3O4 nanocatalyst obtained in Example 2 is shown below.
[0039] Figure 3 The XRD phase characterization diagram of the Ir-doped Co3O4 nanorod catalyst obtained in Example 2 is shown below.
[0040] Figure 4 Here is a high-magnification transmission electron microscopy image of the Ir-doped Co3O4 nanorod catalyst obtained in Example 2;
[0041] Figure 5 XPS phase characterization of the Co 2P orbitals of the Ir-doped Co3O4 nanorod catalyst obtained in Example 2;
[0042] Figure 6 XPS phase characterization of the O1S orbitals of the Ir-doped Co3O4 nanorod catalyst obtained in Example 2. Detailed Implementation
[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. The components of the embodiments of this invention can be arranged and designed in various different configurations.
[0044] The first aspect of this invention provides a method for preparing Ir-doped Co3O4 nanocatalysts, comprising the following steps:
[0045] A. Add an iridium-containing compound solution dropwise to a Co3O4 dispersion at a rate ≤60 μL / min to obtain a mixed solution; after the mixed solution is dried for the first time, a semi-finished Ir-doped Co3O4 nanocatalyst is obtained.
[0046] B. The Ir-doped Co3O4 nanocatalyst semi-finished product is placed in a tube furnace and annealed at 200℃~300℃. After washing and second drying, the Ir-doped Co3O4 nanocatalyst is obtained.
[0047] The preparation method provided by this invention uses spinel oxide Co3O4 as a base material. Co3O4 possesses multiple metal valences, controllable composition, and tunable morphology, playing a crucial role in electron transfer and metal redox cycles. Ir is incorporated into Co3O4 via an impregnation method, increasing the number of active sites in the material. Due to the different electronegativity of Ir and Co, Ir doping induces electron transfer between Ir and Co, adjusting the valence state and electronic structure of Co, thereby modifying the resistance to OH in the OER and ORR processes. - The adsorption and desorption capabilities of the catalyst enhance the reaction energy barrier and improve the catalytic performance of OER and ORR. This preparation method is simple, energy-efficient, and environmentally friendly, improving atom utilization and achieving low loading and high catalytic performance.
[0048] The dropping rate affects the morphology of the formed nanorod catalyst. A dropping rate > 60 μL / min results in uneven solution dispersion, which leads to uneven loading of Ir on Co3O4.
[0049] Typical, but not limiting, dropping rates can be, for example, 20 μL / min, 30 μL / min, 40 μL / min or 50 μL / min.
[0050] Furthermore, the iridium-containing compound includes chloroiridium acid and / or iridium chloride.
[0051] Preferably, the solvent in the iridium-containing compound solution includes water.
[0052] Preferably, the concentration of the iridium-containing compound solution is 10 mg / mL to 40 mg / mL.
[0053] The concentration of the iridium-containing compound solution affects the morphology of the iridium-containing compound in the cobalt oxide dispersion. When the concentration of the iridium-containing compound solution is below 10 mg / mL, the reaction between iridium and cobalt will be incomplete. When the concentration of the iridium-containing compound solution is above 40 mg / mL, the iridium will be unevenly dispersed.
[0054] Typical, but not limiting, concentrations of iridium compound solutions may be, for example, 10 mg / mL, 20 mg / mL, 30 mg / mL, or 40 mg / mL.
[0055] Furthermore, the dispersant of the Co3O4 dispersion includes an alcohol.
[0056] Preferably, the alcohol includes at least one selected from methanol, ethanol, isopropanol, and n-propanol.
[0057] Preferably, the concentration of the Co3O4 dispersion is 1 mg / mL to 3 mg / mL.
[0058] The concentration of the Co3O4 dispersion affects the dispersion state of cobalt oxide. When the concentration of the Co3O4 dispersion is below 1 mg / mL, the reaction will be incomplete; when the concentration of the Co3O4 dispersion is above 3 mg / mL, the Co3O4 will be unevenly dispersed.
[0059] Typical, but not limiting, concentrations of Co3O4 dispersions may be, for example, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, or 3 mg / mL.
[0060] Further, in step A, the mass ratio of the iridium-containing compound to Co3O4 is 0.1 to 1:1, preferably 0.1 to 0.5:1.
[0061] When the mass ratio of iridium-containing compound to Co3O4 is less than 0.1:1, insufficient iridium will lead to the natural loss of raw materials during the synthesis process, resulting in an undetectable Ir content in the final synthesized catalyst, or ultimately, no Ir will be successfully incorporated into Co3O4. When the mass ratio of iridium-containing compound to Co3O4 is greater than 1:1, excessive iridium will further increase the catalyst preparation cost, and will also cause Ir clusters to remain on the surface of Co3O4, preventing them from being incorporated into the crystal lattice to regulate the electronic structure of Co3O4 and adjust the catalyst binding energy.
[0062] Typical, but not limiting, mass ratios of iridium-containing compounds to Co3O4 can be, for example, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, or 1:1.
[0063] Furthermore, the temperature of the first drying process is 60℃~90℃, and the time is 8h~16h.
[0064] Furthermore, in step B, the heating rate is 5°C / min to 10°C / min.
[0065] Preferably, the annealing time is 1 hour to 4 hours.
[0066] In this invention, annealing serves to stabilize the structure of the Ir-doped Co3O4 nanocatalyst. Through the annealing process, Ir can diffuse in Co3O4, making the doping more uniform; it can also promote the entry of Ir into the Co3O4 lattice, increasing the Ir content.
[0067] Typical, but not limiting, annealing temperatures are 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, or 300°C; annealing times can be, for example, 1 hour, 2 hours, 3 hours, or 4 hours.
[0068] Preferably, the washing is performed 3 to 6 times using deionized water.
[0069] Preferably, the second drying is carried out in a vacuum oven, the temperature of which is set to 80℃~120℃ and the time to be 8h~24h.
[0070] The second aspect of the present invention provides an Ir-doped Co3O4 nanocatalyst prepared by the preparation method described above.
[0071] The Ir-doped Co3O4 nanocatalyst provided by this invention incorporates Ir into the Co3O4 lattice, thereby regulating the electronic structure, improving conductivity, and increasing active sites, thus achieving bifunctional catalysis. The ORR half-wave potential of this Ir-doped Co3O4 nanocatalyst is 0.81 V; 10 mA / cm². 2 The OER potential at the current density is 1.488V, and the difference between the two potentials is only 0.678V, which shows excellent bifunctional catalytic activity.
[0072] The third aspect of this invention provides the application of the Ir-doped Co3O4 nanocatalyst in catalytic electrochemical reactions.
[0073] The application of Ir-doped Co3O4 nanocatalysts provided by this invention in catalytic electrochemical reactions offers a catalyst with better performance and multiple functions, reduces the cost of catalyst use, and expands the development of downstream industries.
[0074] Furthermore, the electrochemical reactions include the oxygen evolution reaction (OER) and the oxygen reduction reaction (ORR).
[0075] A fourth aspect of the present invention provides a metal-air battery, comprising an air electrode, a metal electrode, and an electrolyte solution;
[0076] The metal electrode may contain magnesium, aluminum, zinc, mercury or iron.
[0077] A catalyst layer is disposed on the air electrode, and the catalyst in the catalyst layer is the Ir-doped Co3O4 nanocatalyst.
[0078] The metal-air battery provided by this invention has a peak power density of 195 mW / cm³. 2 It also exhibits a cycle stability of up to 1200 hours, making large-scale application of metal-air batteries possible.
[0079] The following detailed description of some embodiments of the present invention is provided in conjunction with examples. Unless otherwise specified, the following embodiments and features can be combined with each other.
[0080] The Co3O4 powder used in the embodiments and comparative examples of this invention was prepared through the following steps:
[0081] (1) Dissolve 0.75 mmol anhydrous cobalt chloride (CoCl2) and 5 mmol urea in 27 mL of ultrapure water, then add 3 mL of glycerol. Place the resulting solution in a 50 mL beaker and stir for 15 min to form a uniformly dispersed mixed solution. Then transfer the mixed solution to a 50 mL reaction vessel and heat it continuously in a 200 °C drying oven for 12 hours.
[0082] (2) After the reaction was completed, the product was washed repeatedly with water and ethanol and centrifuged several times to obtain a precipitate. The precipitate was then dried at 80°C for 12 hours to obtain a Co glycerol ester precursor. The Co glycerol ester precursor was ground and the ground powder was placed in a tube furnace and heated at a rate of 5°C / min. After annealing in air at 350°C for 1 hour, Co3O4 powder was obtained.
[0083] Example 1
[0084] This embodiment provides an Ir-doped Co3O4 nanocatalyst, prepared by the following method:
[0085] (1) Disperse 50 mg of Co3O4 powder in 50 mL of ethanol solution and sonicate for 30 min to obtain a uniformly dispersed Co3O4 dispersion. Add 400 μL of chloroiridium acid solution (concentration of 20 mg / mL) to the Co3O4 dispersion at a rate of 60 μL / min. Then place the mixed solution in an 80 °C drying oven and dry for 12 hours.
[0086] (2) The dried powder was placed in a tube furnace and heated at a rate of 5 °C / min, and annealed in air at 250 °C for two hours. The product was washed with water four times and then dried in a vacuum oven for 12 hours to obtain Ir-doped Co3O4 nanocatalyst.
[0087] Example 2
[0088] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the amount of chloroiridium acid solution added is 600 μL. The other raw materials and methods are the same as in Example 1, and will not be repeated here.
[0089] Example 3
[0090] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the amount of chloroiridium acid solution added is 800 μL. The other raw materials and methods are the same as in Example 1, and will not be repeated here.
[0091] Example 4
[0092] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the amount of chloroiridium acid solution added is 2.5 mL. The other raw materials and methods are the same as in Example 1, and will not be repeated here.
[0093] Example 5
[0094] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the concentration of the Co3O4 dispersion is 0.1 mg / mL; the concentration of the chloroiridium acid solution is 10 mg / mL; and the other raw materials and methods are the same as in Example 1, which will not be repeated here.
[0095] Example 6
[0096] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the concentration of the Co3O4 dispersion is 3 mg / mL; the concentration of the chloroiridium acid solution is 40 mg / mL; and the remaining raw materials and methods are the same as in Example 1, which will not be repeated here.
[0097] Example 7
[0098] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that the concentration of the Co3O4 dispersion is 10 mg / mL; the concentration of the chloroiridium acid solution is 50 mg / mL; and the remaining raw materials and methods are the same as in Example 1, which will not be repeated here.
[0099] Example 8
[0100] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that in step 2, the nanocatalyst is annealed in air at 350°C for two hours. The other raw materials and methods are the same as in Example 1, and will not be repeated here.
[0101] Example 9
[0102] This embodiment provides an Ir-doped Co3O4 nanocatalyst. The difference from Example 1 is that in step 2, the nanocatalyst is annealed in air at 150°C for two hours. The other raw materials and methods are the same as in Example 1, and will not be repeated here.
[0103] Comparative Example 1
[0104] This comparative example provides a Co3O4 nanocatalyst, which has the same source as the Co3O4 powder in the examples.
[0105] Comparative Example 2
[0106] This comparative example provides an Ir / C catalyst, which is a commercial OER (oxygen evolution reaction) catalyst.
[0107] Comparative Example 3
[0108] This comparative example provides a Pt / C catalyst, which is a commercial oxygen reduction reaction (ORR) catalyst.
[0109] Characterization Example 1
[0110] The morphology of the Ir-doped Co3O4 nanocatalyst obtained in Example 2 was observed under a high-magnification transmission electron microscope, and the morphology image is shown below. Figure 1 As shown.
[0111] from Figure 1 As can be seen, Example 2 successfully synthesized a catalyst with a nanorod morphology.
[0112] Characterization Example 2
[0113] The elemental distribution characterization diagram of the Ir-doped Co3O4 nanocatalyst obtained in Example 2 is shown below. Figure 2 As shown.
[0114] from Figure 2 As can be seen from the elemental distribution diagram, Ir is uniformly distributed in Co3O4, and its content is much lower than that of Co and O, which confirms that Ir has been successfully doped into Co3O4. Figure 2 The single-element distribution map shows the three elements Co, O, and Ir in that order.
[0115] Characterization Example 3
[0116] The Ir-doped Co3O4 nanocatalyst obtained in Example 2 was subjected to XRD and high-magnification transmission electron microscopy, and the results are as follows: Figure 3 and Figure 4 As shown.
[0117] from Figure 3 As can be seen from the XRD phase characterization diagram of the Ir-doped Co3O4 nanorod catalyst, the XRD pattern shows that the crystal structure of Co3O4 was maintained after Ir doping, and no new diffraction peaks appeared, indicating that no new crystal phase was formed after doping. However, the peak intensity decreased, and the crystallinity deteriorated. This is because the Ir doping affected the crystal structure of Co3O4.
[0118] Figure 4The image shows the high-magnification transmission electron microscopy (TEM) morphology of the Ir-doped Co3O4 nanorod catalyst. The TEM image reveals clear lattice fringes with dimensions of 0.24 nm and 0.463 nm, corresponding to the 311 and 111 crystal planes of Co3O4, respectively, which is consistent with the XRD test results.
[0119] Characterization Example 4
[0120] XPS was performed on the Ir-doped Co3O4 nanocatalyst obtained in Example 2.
[0121] Figure 5 The XPS phase characterization diagram of the Co 2P orbitals of the Ir-doped Co3O4 nanorod catalyst shows four main peaks corresponding to Co. 2+ Co 3+ The Ir-doped Co3O4 nanorod catalyst was compared with Comparative Example 1, and the results showed that Co 3+ Peak area and Co 2 + The increase in the ratio from 35.9% to 38.4% indicates that electron transfer occurred between Ir and Co3O4, adjusting the valence state of Co3O4 and leading to Co 3+ The increase in this factor improves OER performance.
[0122] Figure 6 XPS phase characterization of the O1S orbitals of the Ir-doped Co3O4 nanorod catalyst. The spectrum shows that after Ir doping, the proportion of oxygen vacancies increased from 15.9% to 17%. The increased oxygen vacancies optimized the adsorption energy of reactants on the catalyst surface, thereby reducing the reaction energy barrier, promoting molecular activation, and improving the catalytic performance of OER and ORR.
[0123] Test Example 1
[0124] Electrochemical performance polarization curves were tested for the catalysts of Examples 1-9 and Comparative Examples 1-3.
[0125] The specific process is as follows:
[0126] Catalyst ink preparation: Take 2 mg of catalyst, 600 μL of ethanol, 200 μL of deionized water, and 5 μL of Nafion (perfluorosulfonic acid) and place them in a centrifuge tube. Sonicate for at least 30 minutes.
[0127] During OER testing, 80 μL of catalyst ink was drop-coated onto a 1 cm × 1 cm carbon cloth, resulting in a catalyst loading of 0.2 mg / cm². -2After natural drying, the sample was used as the working electrode, a calomel electrode as the reference electrode, and a platinum sheet as the counter electrode. Testing was conducted in an oxygen-saturated 1M KOH solution. All samples were tested on an Ivium workstation. The voltage range for CV testing was 0–0.5 V, and the scan rate was 50 mV / s. The voltage range for LSV testing was 0–0.8 V, and the scan rate was 5 mV / s.
[0128] During ORR testing, 15 μL of catalyst ink was added three times to a rotating disk electrode as the working electrode, with a catalyst loading of 0.3 mg / cm³. 2 A calomel electrode was used as the reference electrode, and a platinum wire as the counter electrode. Tests were conducted in an oxygen-saturated 1 MkOH solution. All tests were performed on a CHI 660E electrochemical workstation. The voltage range for CV tests was -0.9 to -0.1 V, with a scan rate of 50 mV / s. The voltage range for LSV tests was -1.1 to 0 V, with a scan rate of 5 mV / s, and the rotating disk electrode was rotated at 1600 rpm.
[0129] The obtained data is shown in Table 1 below.
[0130] The overpotential of OER is 10 mA / cm. 2 The results were obtained from tests conducted at current density.
[0131] Table 1
[0132]
[0133]
[0134] As can be seen from Table 1, the catalysts in Examples 1-9 have a performance of 10 mA / cm². 2 The voltage difference ΔE between the potential at current density and the ORR half-wave potential is only 0.66V, which is better than commercial Pt / C and Ir / C catalysts.
[0135] Test Example 2
[0136] 400 μL of catalyst ink was drop-coated onto carbon cloth to serve as an air cathode. Before use, the carbon cloth was ultrasonically treated for 30 minutes each in acetone, ethanol, and ultrapure water. The catalyst coating area was 1 square centimeter, and the catalyst loading was 1 mg / cm². 2Polished zinc sheets were used as the negative electrode, and the electrolyte consisted of 6M KOH and 0.2M Zn(Ac)₂. A 3 square centimeter zinc-air battery membrane was used, assembled layer by layer in the following order: a water-permeable membrane, nickel foam, carbon cloth with catalyst support, a waterproof separator, and finally the zinc sheet. Testing was conducted on a CHI1140E electrochemical workstation. The discharge test voltage range was 1.6V–0.2V, with a scan rate of 5mV / s. The charge test voltage range was 1.6V–3V, with a scan rate of 5mV / s. Charge-discharge cycles were performed at 10mA / cm². 2 The process is carried out at a specific current density, with one cycle consisting of 15 minutes of charging and 15 minutes of discharging.
[0137] The obtained data is shown in Table 2 below.
[0138] Table 2
[0139]
[0140]
[0141] As shown in Table 2, the peak power density of the liquid zinc-air batteries assembled using the catalysts in Examples 1-9 as air cathodes reached as high as 198 mW / cm². 2 It also has a charge-discharge cycle life of up to 1200 hours, which is superior to Pt / C and Ir / C mixed catalysts.
[0142] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing Ir-doped Co3O4 nanocatalysts for catalyzing electrochemical reactions, characterized in that, Includes the following steps: A. An iridium-containing compound solution is added dropwise to a Co3O4 dispersion, wherein the dispersant of the Co3O4 dispersion includes an alcohol, the mass ratio of the iridium-containing compound to Co3O4 is 0.1 to 1:1, and the dropping rate is ≤60 μL / min, to obtain a mixed solution; the mixed solution is dried first to obtain a semi-finished Ir-doped Co3O4 nanocatalyst. B. The Ir-doped Co3O4 nanocatalyst semi-finished product is placed in a tube furnace and annealed at 200℃~300℃ with a heating rate of 5℃ / min~10℃ / min. After washing and second drying, the Ir-doped Co3O4 nanocatalyst is obtained, and the catalyst has a nanorod morphology.
2. The preparation method according to claim 1, characterized in that, The iridium-containing compounds include chloroiridium acid and / or iridium chloride.
3. The preparation method according to claim 2, characterized in that, The solvent in the iridium-containing compound solution includes water.
4. The preparation method according to claim 3, characterized in that, The concentration of the iridium-containing compound solution is 10 mg / mL to 40 mg / mL.
5. The preparation method according to claim 4, characterized in that, The alcohol includes at least one of methanol, ethanol, isopropanol, and n-propanol.
6. The preparation method according to claim 4, characterized in that, The concentration of the Co3O4 dispersion is 1 mg / mL to 3 mg / mL.
7. The preparation method according to claim 1, characterized in that, The mass ratio of the iridium-containing compound to Co3O4 is 0.1 to 0.5:
1.
8. The preparation method according to any one of claims 1 to 7, characterized in that, The first drying temperature is 60℃~90℃, and the time is 8h~16h.
9. The preparation method according to any one of claims 1 to 7, characterized in that, The annealing time is 1 hour to 4 hours.
10. The preparation method according to any one of claims 1 to 7, characterized in that, The washing process is performed 3 to 6 times using deionized water.
11. The preparation method according to any one of claims 1 to 7, characterized in that, The second drying is carried out in a vacuum oven, with the temperature set to 80℃~120℃ and the time to be 8h~24h.
12. An Ir-doped Co3O4 nanocatalyst prepared by the preparation method according to any one of claims 1 to 11.
13. The application of the Ir-doped Co3O4 nanocatalyst according to claim 12 in catalytic electrochemical reactions.
14. The application according to claim 13, characterized in that, The electrochemical reactions include the oxygen evolution reaction and the oxygen reduction reaction.
15. A metal-air battery, characterized in that, Includes air electrode, metal electrode and electrolyte solution; The metal electrode may contain magnesium, aluminum, zinc, mercury or iron. The air electrode is provided with a catalyst layer, and the catalyst in the catalyst layer is an Ir-doped Co3O4 nanocatalyst prepared by the preparation method according to any one of claims 1 to 11.
Citation Information
Patent Citations
Platinum group metal catalyst and preparation and application thereof
CN114917927A