A preparation method and recycling method of high-strength thermoplastic elastomer material
Through the process of generating a heterogeneous crosslinking network in TPV and introducing zinc salt ion bonds, the problem of insufficient mechanical properties of TPV is solved, significantly improved its strength and toughness, and achieved good recyclable performance, supporting the rubber industry Green development.
Patent Information
- Application Number
- CN202311731369.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-12-15
AI Technical Summary
The existing thermoplastic vulcanized rubber (TPV) have problems with insufficient toughness and strength in terms of mechanical properties, especially because the compatibility between polyamide 6 (PA6) and rubber is poor, which makes it difficult to meet the actual engineering application needs.
Using a non-filling enhancement method, high-strength TPV is prepared by generating a process with a heterogeneous crosslinking network and introducing zinc salt ion bonds. The specific steps include reacting the rubber with an excess vulcanizing agent to form a fully vulcanized rubber powder, mixing unvulcanized rubber and fully vulcanized rubber, adding zinc oxide and maleic acid to form a zinc salt ion bond, and dynamically vulcanized with the plastic to form a heterogeneous network and zinc salt. High-strength TPV of ionic bonds.
The tensile strength, elongation of break and elastic modulus of TPV are significantly improved, and the tensile strength, elongation of break and elastic modulus are increased by 109.2%, 338.34% and 51.5% compared with ordinary PA6/NBR-based TPV, respectively, and have good recyclable performance, supporting the rubber industry Green development.
Smart Images

Figure CN117683180B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material processing, and in particular relates to a preparation method and a recovery method of a high-toughness thermoplastic elastomer material. Background Art
[0002] Thermoplastic vulcanizate (TPV) is a high-performance elastomer, which is made by dynamic vulcanization technology with a small amount of plastic as the continuous phase and a large amount of highly cross-linked rubber particles as the dispersed phase. Due to the combination of the high elasticity of rubber and the recyclability of thermoplastics, TPV is called "green rubber" and is widely used in automobiles, sensors, acoustic materials and other fields.
[0003] In order to meet various industrial applications, TPV generally needs to be reinforced. Since polyamide 6 (PA6) has excellent engineering properties, TPV prepared with PA6 as the plastic phase has become one of the most common commercial TPVs. However, the mechanical properties of TPV are not only related to the properties of the raw materials themselves, but also affected by the compatibility between rubber and plastic. Due to the strong polarity of PA6, the compatibility between PA6 and rubber is poor, which leads to low strength and toughness of TPV, making it difficult to meet actual engineering applications. Therefore, effective reinforcement methods are needed to improve the mechanical properties of PA6-based TPV.
[0004] The most common method of reinforcing rubber is to compound various nanoparticles (NPs) into the rubber matrix, such as carbon black (CB), silica, carbon nanotubes (CNTs), etc. However, nanofilling is largely limited by processing difficulties, dispersion / interface fine adjustment, and dynamic hysteresis / heating. In recent years, various non-filling reinforcement methods have been rapidly developed. For example, reversible bonds such as hydrogen bonds, ionic bonds, metal-ligand interactions, and molecular interdiffusion are introduced into rubber to improve its strength and fracture toughness. At the same time, the reversible dissociation / association of these bonds during deformation can maintain the integrity of the network. In addition, effective reinforcement of rubber can also be achieved by controlling the distribution of long and short chains in the rubber cross-linked network. In this heterogeneous network, short chains mainly increase the modulus through their limited deformation ability, while long chains inhibit the propagation of cracks to a certain extent, avoiding catastrophic damage to the network. Non-filling methods can effectively make up for the shortcomings of filling methods while improving the fracture toughness and resilience of rubber and avoiding the loss of dynamic mechanical properties.
[0005] In recent years, research on non-filler reinforcement methods has mainly focused on vulcanized rubber materials, and there is less research on how to enhance TPV through non-filler methods. How to reasonably use non-filler reinforcement methods to prepare high-performance TPVs remains to be explored.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a preparation method and a recycling method of a high-strength and tough thermoplastic elastomer material.
[0008] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0009] A method for preparing a high-toughness thermoplastic elastomer material comprises the following steps:
[0010] Step (1): reacting rubber with an excess amount of a vulcanizing agent to produce fully vulcanized rubber powder;
[0011] The method for producing fully vulcanized rubber powder in step (1) is as follows:
[0012] Step (1.1): First, add the rubber into the internal mixer and set the rotor speed and temperature;
[0013] Step (1.2): Add vulcanizing agent and continue melting reaction and mixing until the torque is stable to obtain fully vulcanized rubber powder
[0014] Step (2): mixing rubber powder with unvulcanized rubber to obtain a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network;
[0015] The method for preparing the rubber having a heterogeneous cross-linked network in step (2) is as follows:
[0016] Step (2.1): uniformly mixing unvulcanized rubber and fully vulcanized rubber powder in a weight ratio of 3:1 to prepare a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network;
[0017] Step (3): mixing maleic acid and zinc oxide in a heterogeneous cross-linked network rubber, reacting in situ to generate zinc maleate having a zinc salt ionic bond, and obtaining a rubber masterbatch having a heterogeneous network and zinc maleate;
[0018] The method for preparing zinc maleate having zinc salt ionic bond in step (3) is as follows:
[0019] Step (3.1): adding the rubber masterbatch having a heterogeneous cross-linked network into an internal mixer, and setting the speed and stability of the rotor;
[0020] Step (3.2): adding zinc oxide in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network;
[0021] Step (3.3): adding maleic acid in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network to react and generate a rubber having a heterogeneous network and zinc maleate;
[0022] Step (3.4): when the torque value reaches a stable value, taking the rubber having the heterogeneous network and zinc maleate out of the cavity of the internal mixer and cooling it to a temperature to obtain a rubber masterbatch having the heterogeneous network and zinc maleate;
[0023] Step (4): preparing TPV using a rubber masterbatch and plastic having a heterogeneous network and zinc maleate, and adding peroxide to polymerize and graft the zinc maleate, thereby obtaining a high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds, and finally preparing a dumbbell-shaped specimen of the high-strength and tough TPV;
[0024] The method for preparing a high-strength and tough TPV having a heterogeneous network and zinc salt ionic bonds in step (4) is as follows:
[0025] Step (4.1): adding a rubber masterbatch having a heterogeneous network and zinc maleate and a plastic having a rubber-plastic ratio of 50:50 into an internal mixer in sequence, setting the speed and temperature of the rotor to generate a blend of the rubber masterbatch having a heterogeneous network and zinc maleate and the plastic;
[0026] Step (4.2): adding a vulcanizing agent for dynamic vulcanization of the blend;
[0027] Step (4.3): When the torque is stable, peroxide is added for polymerization and grafting of zinc maleate;
[0028] Step (4.4): taking out the generated high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds from the internal mixer;
[0029] Step (4.5): forming a high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds at 230° C. and 5 MPa to prepare a sheet having a thickness of about 2.0 mm, and cutting out a dumbbell-shaped specimen;
[0030] Step (5): preparing TPV (H-TPV) and ordinary TPV (TPV) with only a heterogeneous cross-linked network as a control group, and conducting a control experiment with the high-strength and tough TPV dumbbell-shaped specimen;
[0031] The preparation process of the H-TPV control group in step (5) is as follows:
[0032] Step (5.1): H-NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added to an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of the H-NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of the H-NBR are added for dynamic vulcanization of the blend. When the torque is stable, the H-TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a thin plate with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0033] In step (5.1), the rotor speed of the internal mixer is set to 80 rpm and the temperature is set to 230°C;
[0034] The preparation process of the TPV control group in step (5) is as follows:
[0035] Step (5.2): NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added to an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of NBR are added for dynamic vulcanization of the blend. When the torque is stable, the TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a sheet with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0036] In step (5.2), the rotor speed of the internal mixer is set to 80 rpm and the temperature is set to 230°C;
[0037] A method for recycling a high-toughness thermoplastic elastomer material comprises the following steps:
[0038] Step 1: Take the used high-strength and tough TPV with a heterogeneous network and zinc salt ionic bonds, and process the high-strength and tough TPV with a heterogeneous network and zinc salt ionic bonds to crush them;
[0039] Step 2: Then add it to the blender for processing;
[0040] A specific recycling method of a high-strength and tough thermoplastic elastomer material is as follows: a thin plate sample is cut into small pieces and then added to a stirrer at a rotor speed of 80 rpm and a set temperature of 230°C for 5 minutes. After that, the melted sample is hot-pressed at the same temperature for another 5 minutes. After the tensile test is completed, the reprocessed sample is recycled to the next generation again;
[0041] The elongation at break of the samples without reversible Zn2+ salt bonds decreased dramatically, while MH-TPV maintained excellent mechanical properties after repeated cycles.
[0042] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time:
[0043] The present invention adopts two non-filling reinforcement methods, including establishing a heterogeneous cross-linked network and introducing zinc salt ionic bonds, and prepares a high-strength PA6 / NBR-based TPV through a simple process flow. This high-strength TPV has excellent mechanical properties, and its tensile strength, elongation at break and elastic modulus reach 21.2MPa, 221.2% and 197MPa, respectively, which are 109.2%, 338.34% and 51.5% higher than those of ordinary PA6 / NBR-based TPV, respectively, and the improvement effect is significant.
[0044] Normally, when TPV is stretched, the dispersed rubber phase will pull back the deformed plastic matrix nearby through its elasticity, thus avoiding the overall breakage of TPV. In high-strength and tough TPV with heterogeneous network and zinc salt ionic bond, the good adhesion provided by zinc salt ionic bond between NBR and PA6 will allow NBR particles to absorb the applied mechanical energy, while the fully vulcanized NBR provides higher strength and elasticity to the rubber phase, which can provide higher strength and toughness to TPV;
[0045] Secondly, this high-strength and tough TPV with both a heterogeneous network and zinc salt ionic bonds has good recyclability. The recycling method is completed by extrusion, which can be produced stably and continuously without the use of any special processing equipment. The recovered rubber has a high recovery rate, which is of great significance to the green development of the rubber industry.
[0046] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The drawings described below are only some embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0048] Figure 1 A schematic diagram of a preparation process according to an embodiment of the present invention;
[0049] Figure 2 A comparison chart of the mechanical properties of the high-toughness TPV and other TPVs according to an embodiment of the present invention;
[0050] Figure 3 A microstructure diagram and a tensile schematic diagram of a high-toughness TPV according to an embodiment of the present invention;
[0051] Figure 4 A schematic diagram of a recycling process according to an embodiment of the present invention;
[0052] Figure 5 This is a schematic diagram of mechanical properties comparison after recycling cycle of an embodiment of the present invention;
[0053] Figure 6is a flow chart of a preparation process according to an embodiment of the present invention;
[0054] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. Implementation
[0055] The present invention will now be described in further detail with reference to the accompanying drawings. Example
[0056] A method for preparing a high-toughness thermoplastic elastomer material comprises the following steps:
[0057] Step (1): reacting rubber with an excess amount of a vulcanizing agent to produce fully vulcanized rubber powder;
[0058] The method for producing fully vulcanized rubber powder in step (1) is as follows:
[0059] Step (1.1): first, add the rubber into the torque mixer and set the rotor speed and temperature;
[0060] Step (1.2): Add vulcanizing agent and continue melting reaction and mixing until the torque is stable to obtain fully vulcanized rubber powder
[0061] Step (2): mixing rubber powder with unvulcanized rubber to obtain a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network;
[0062] The method for preparing the rubber having a heterogeneous cross-linked network in step (2) is as follows:
[0063] Step (2.1): uniformly mixing unvulcanized rubber and fully vulcanized rubber powder in a weight ratio of 3:1 to prepare a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network;
[0064] Step (3): mixing maleic acid and zinc oxide in a heterogeneous cross-linked network rubber, reacting in situ to generate zinc maleate having a zinc salt ionic bond, and obtaining a rubber masterbatch having a heterogeneous network and zinc maleate;
[0065] The method for preparing zinc maleate having zinc salt ionic bond in step (3) is as follows:
[0066] Step (3.1): adding the rubber masterbatch having a heterogeneous cross-linked network into an internal mixer, and setting the speed and stability of the rotor;
[0067] Step (3.2): adding zinc oxide in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network;
[0068] Step (3.3): adding maleic acid in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network to react and generate a rubber having a heterogeneous network and zinc maleate;
[0069] Step (3.4): when the torque value reaches a stable value, taking the rubber having the heterogeneous network and zinc maleate out of the cavity of the internal mixer and cooling it to a temperature to obtain a rubber masterbatch having the heterogeneous network and zinc maleate;
[0070] Step (4): preparing TPV using a rubber masterbatch and plastic having a heterogeneous network and zinc maleate, and adding peroxide to polymerize and graft the zinc maleate, thereby obtaining a high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds, and finally preparing a dumbbell-shaped specimen of the high-strength and tough TPV;
[0071] The method for preparing a high-strength and tough TPV having a heterogeneous network and zinc salt ionic bonds in step (4) is as follows:
[0072] Step (4.1): adding a rubber masterbatch having a heterogeneous network and zinc maleate and a plastic having a rubber-plastic ratio of 50:50 into an internal mixer in sequence, setting the speed and temperature of the rotor to generate a blend of the rubber masterbatch having a heterogeneous network and zinc maleate and the plastic;
[0073] Step (4.2): adding a vulcanizing agent for dynamic vulcanization of the blend;
[0074] Step (4.3): When the torque is stable, peroxide is added for polymerization and grafting of zinc maleate;
[0075] Step (4.4): taking out the generated high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds from the internal mixer;
[0076] Step (4.5): forming a high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds at 230° C. and 5 MPa to prepare a sheet having a thickness of about 2.0 mm, and cutting out a dumbbell-shaped specimen;
[0077] Step (5): preparing TPV (H-TPV) and ordinary TPV (TPV) with only a heterogeneous cross-linked network as a control group, and conducting a control experiment with the high-strength and tough TPV dumbbell-shaped specimen;
[0078] The preparation process of the control group of TPV (H-TPV) having only a heterogeneous cross-linked network in step (5) is as follows:
[0079] Step (5.1): H-NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added to an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of the H-NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of the H-NBR are added for dynamic vulcanization of the blend. When the torque is stable, the H-TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a thin plate with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0080] In step (5.1), the rotor speed of the internal mixer is set to 80 rpm and the temperature is set to 230°C;
[0081] The preparation process of the TPV control group in step (5) is as follows:
[0082] Step (5.2): NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added to an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of NBR are added for dynamic vulcanization of the blend. When the torque is stable, the TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a sheet with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0083] The rubber in this embodiment may be NBR, EPDM, or NR, the plastic may be PA6 or PP, and the vulcanizing agent may be PF or sulfur.
[0084] In step (5.2), the rotor speed of the internal mixer is set to 80 rpm and the temperature is set to 230°C;
[0085] A method for recycling a high-toughness thermoplastic elastomer material comprises the following steps:
[0086] Step 1: Take the used high-strength and tough TPV with a heterogeneous network and zinc salt ionic bonds, and process the high-strength and tough TPV with a heterogeneous network and zinc salt ionic bonds to crush them;
[0087] Step 2: Then add it to the blender for processing;
[0088] A specific recycling method of a high-strength and tough thermoplastic elastomer material is as follows: a thin plate sample is cut into small pieces and then added to a stirrer at a rotor speed of 80 rpm and a set temperature of 230°C for 5 minutes. After that, the melted sample is hot-pressed at the same temperature for another 5 minutes. After the tensile test is completed, the reprocessed sample is recycled to the next generation again;
[0089] The elongation at break of the sample without zinc salt ionic bonds dropped dramatically, while the high-strength and tough TPV with heterogeneous network and zinc salt ionic bonds maintained excellent mechanical properties after repeated cycles.
[0090] Implementation 2:
[0091] A method for preparing a high-toughness thermoplastic elastomer material comprises the following steps:
[0092] S1: Use excess vulcanizing agent to react with NBR to generate fully vulcanized NBR powder;
[0093] The method for producing fully vulcanized NBR powder in S1 is as follows:
[0094] S1.1: First, add NBR into the internal mixer, set the rotor speed to 120 rpm and the temperature to 160°C;
[0095] S1.2: After 5 minutes, phenolic resin powder with a mass ratio of 8wt% of the total weight of NBR and stannous chloride with a mass ratio of 0.6wt% of the total weight of NBR were added, and the melting reaction and mixing were continued until the torque was stable to obtain an NBR sample, which was named fully vulcanized NBR;
[0096] S2: Mixing fully vulcanized NBR with pure NBR to obtain a rubber masterbatch H-NBR with a heterogeneous cross-linking network;
[0097] The method for preparing the rubber masterbatch H-NBR in S2 is as follows:
[0098] S2.1: NBR and fully vulcanized NBR are uniformly mixed in a weight ratio of 3:1 to prepare H-NBR as the rubber phase of the TPV;
[0099] S3: zinc oxide and maleic acid are sequentially added to the rubber masterbatch H-NBR to react in situ to generate zinc maleate. When the torque value reaches a stable value, the rubber masterbatch H-NBR is taken out from the cavity of the internal mixer and cooled, and is named MH-NBR;
[0100] The method for preparing MH-NBR in S3 is as follows:
[0101] S3.1: Add H-NBR into the internal mixer, set the rotor speed to 80 rpm and the temperature to 140°C;
[0102] S3.2: After 3 minutes, zinc oxide in an amount of 5 wt% of the total weight of H-NBR is added;
[0103] S3.3: After 5 minutes, maleic acid (5 wt% of the total weight of H-NBR) is added to react to form zinc maleate;
[0104] S3.4: When the torque value reaches a stable value, the H-NBR is taken out from the cavity of the internal mixer and cooled to the temperature, and is named MH-NBR;
[0105] S4: The prepared rubber masterbatch MH-NBR and PA6 were made into TPV by dynamic vulcanization technology, and peroxide was added to polymerize and graft the zinc maleate in the rubber masterbatch to obtain a high-strength and tough TPV named MH-TPV. Finally, a dumbbell-shaped specimen of MH-TPV was made;
[0106] The method for preparing MH-TPV in S4 is as follows:
[0107] S4.1: Add MH-NBR and PA6 with a rubber-plastic ratio of 50:50 into an internal mixer in sequence, set the rotor speed to 80 rpm and the temperature to 230°C;
[0108] S4.2: adding phenolic resin powder in a mass ratio of 4wt% of the total weight of MH-NBR and stannous chloride in a mass ratio of 0.2wt% of the total weight of MH-NBR for dynamic vulcanization of the blend;
[0109] S4.3: When the torque is stable, dicumyl peroxide is added in a mass ratio of 1 wt% of the total weight of MH-NBR for polymerization and grafting of zinc maleate;
[0110] S4.4: After 3 minutes, the generated MH-TPV is taken out from the internal mixer;
[0111] S4.5: forming the MH-TPV at 230°C and 5 MPa to prepare a sheet with a thickness of about 2.0 mm, and cutting out dumbbell-shaped specimens;
[0112] S5: TPV with only heterogeneous cross-linked network (H-TPV) and ordinary TPV (TPV) were prepared as the control group and compared with MH-TPV dumbbell-shaped specimens for control experiments;
[0113] The preparation process of the control group of TPV (H-TPV) with only a heterogeneous cross-linked network in S5 is as follows:
[0114] S5.1: H-NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added into an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of H-NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of H-NBR are added for dynamic vulcanization of the blend. When the torque is stable, the H-TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a sheet with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0115] In S5.1, the internal mixer is set to a rotor speed of 80 rpm and a temperature of 230°C;
[0116] The preparation process of the TPV control group in S5 is as follows:
[0117] S5.2: NBR and PA6 with a rubber-plastic ratio of 50:50 are sequentially added into an internal mixer, and then phenolic resin powder with a mass ratio of 4wt% of the total weight of NBR and stannous chloride with a mass ratio of 0.2wt% of the total weight of NBR are added for dynamic vulcanization of the blend. When the torque is stable, the TPV is taken out of the internal mixer and molded at 230°C and 5MPa to prepare a sheet with a thickness of about 2.0mm, and a dumbbell-shaped specimen is cut out;
[0118] In S5.2, the internal mixer is set to a rotor speed of 80 rpm and a temperature of 230°C.
[0119] According to ISO37-2005 standard, the dumbbell specimens were subjected to uniaxial tensile tests at a speed of 10 mm / min using an Instron universal testing machine (Instron, model 5567). At least five specimens were used for each measurement, and the average value was taken and plotted into a stress-strain curve. And according to the formula: The elastic modulus of the material under quasi-elastic deformation is obtained, where E is the elastic modulus, σ is the stress, and ε is the strain.
[0120] like Figure 2 As shown, the comparative data of mechanical properties:
[0121] A method for recovering MH-TPV comprises the following steps:
[0122] rubber Tensile Strength Elongation at break Elastic modulus TPV 10.1MPa 45.30% 130MPa H-TPV 13.5MPa 134.20% 138MPa MH-TPV 21.2MPa 221.20% 197MPa
[0123] Step 1: Take the used MH-TPV and cut it into small pieces;
[0124] Step 2: Then add it to the blender for processing;
[0125] Step 3: The melted samples were hot pressed again at the same temperature for 5 minutes. After the tensile test was completed, the processed samples were recycled to the next generation;
[0126] like Figure 4 As shown in Figure 1, the specific recycling method of MH-TPV is as follows: the sheet sample is cut into small pieces and then added to the mixer at a rotor speed of 80 rpm and a set temperature of 230 ° C for 5 minutes. After that, the melted sample is hot pressed at the same temperature for another 5 minutes. After the tensile test is completed, the reprocessed sample is recycled to the next generation again;
[0127] The elongation at break of the sample without Zn2+ salt reversible bond dropped sharply, while MH-TPV still maintained excellent mechanical properties after repeated cycles.
[0128] As for raw materials, the brand of NBR is DN003; the brand of PA6 is B3S; the brand of phenolic resin is SP-1045; stannous chloride is purchased from China McLean Biochemical Industry Company; zinc oxide, maleic acid and diisopropylbenzene peroxide are all purchased from China National Pharmaceutical Group Chemical Reagent Co., Ltd.
[0129] like Figure 5 Shown: Comparison of mechanical properties after recycling:
[0130] TPV H-TPV MH-TPV Initial performance Tensile Strength 10.1MPa 13.5MPa 21.2MPa Elongation at break 45.30% 134.20% 221.20% First cycle Tensile Strength 10.4MPa 15.8MPa 21.6MPa Elongation at break 24.90% 60.30% 218.10% Second cycle Tensile Strength 10.5MPa 14.1MPa 20.8MPa Elongation at break 14.90% 26.60% 228.80% Third cycle Tensile Strength 6.8MPa 16.4MPa 20.8MPa Elongation at break 16.60% 38.50% 209.10%
[0131] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. A method for preparing a high-toughness thermoplastic elastomer material, characterized in that: The following steps are involved: Step (1): reacting rubber with an excess amount of a vulcanizing agent to produce fully vulcanized rubber powder; The method for producing fully vulcanized rubber powder in step (1) is as follows: Step (1.1): First, add the rubber into the internal mixer and set the rotor speed and temperature; Step (1.2): Add vulcanizing agent, continue melting reaction and mixing until the torque is stable, and obtain fully vulcanized rubber powder; Step (2): mixing rubber powder with unvulcanized rubber to obtain a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network; The method for preparing the rubber having a heterogeneous cross-linked network in step (2) is as follows: Step (2.1): uniformly mixing 60%-80% of unvulcanized rubber and 20%-40% of fully vulcanized rubber powder to prepare a rubber having a heterogeneous cross-linked network as a rubber masterbatch having a heterogeneous cross-linked network; Step (3): mixing maleic acid and zinc oxide in a heterogeneous cross-linked network rubber, reacting in situ to generate zinc maleate having a zinc salt ionic bond, and obtaining a rubber masterbatch having a heterogeneous network and zinc maleate; Wherein, the method for preparing zinc maleate having zinc salt ionic bond in step (3) is as follows: Step (3.1): adding the rubber masterbatch having a heterogeneous cross-linked network into an internal mixer, and setting the speed and stability of the rotor; Step (3.2): adding zinc oxide in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network; Step (3.3): adding maleic acid in an amount of 5 wt% of the total weight of the rubber masterbatch having a heterogeneous cross-linked network to react and generate a rubber having a heterogeneous network and zinc maleate; Step (3.4): when the torque value reaches a stable value, taking the rubber having the heterogeneous network and zinc maleate out of the cavity of the internal mixer and cooling it to a temperature to obtain a rubber masterbatch having the heterogeneous network and zinc maleate; Step (4): preparing TPV using a rubber masterbatch and plastic having a heterogeneous network and zinc maleate, and adding peroxide to polymerize and graft the zinc maleate, thereby obtaining a high-strength and tough TPV (MH-TPV) having both a heterogeneous network and zinc salt ionic bonds, and finally preparing a dumbbell-shaped specimen of the high-strength and tough TPV; The method for preparing a high-strength and tough TPV having a heterogeneous network and zinc salt ionic bonds in step (4) is as follows: Step (4.1): adding the rubber masterbatch having a heterogeneous network and zinc maleate and the plastic into an internal mixer in sequence, setting the speed and temperature of the rotor, and generating a blend of the rubber masterbatch having a heterogeneous network and zinc maleate and the plastic; Step (4.2): adding a vulcanizing agent for dynamic vulcanization of the blend; Step (4.3): When the torque is stable, peroxide is added for polymerization and grafting of zinc maleate; Step (4.4): taking out the generated high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds from the internal mixer; Step (4.5): forming a high-strength and tough TPV having both a heterogeneous network and zinc salt ionic bonds at 230° C. and 5 MPa to prepare a sheet having a thickness of about 2.0 mm, and cutting out a dumbbell-shaped specimen; Step (5): preparing TPV (H-TPV) having only a heterogeneous cross-linked network and ordinary TPV (TPV) as a control group, and conducting a control experiment with the high-strength and tough TPV dumbbell-shaped specimen; The preparation process of the control group of TPV (H-TPV) having only a heterogeneous cross-linked network in step (5) is as follows: Step (5.1): adding the rubber (H-NBR) having only a heterogeneous cross-linked network and PA6 to an internal mixer in sequence, and then adding phenolic resin powder accounting for 4 wt% of the total weight of the H-NBR and stannous chloride accounting for 0.2 wt% of the total weight of the H-NBR for dynamic vulcanization of the blend. When the torque is stable, the H-TPV is taken out of the internal mixer and molded at 230° C. and 5 MPa to prepare a sheet with a thickness of about 2.0 mm, and a dumbbell-shaped specimen is cut out; The preparation process of the rubber (H-NBR) having only a heterogeneous cross-linked network in step (5.1) is as follows: NBR and fully vulcanized NBR are uniformly mixed in a weight ratio of 3:1 to prepare H-NBR; Wherein, in step (5.1), the rotor speed of the internal mixer is set to 80 rpm and the temperature is set to 230°C; The preparation process of the TPV control group in step (5) is as follows: Step (5.2): NBR and PA6 are sequentially added to an internal mixer, and then phenolic resin powder with a mass ratio of 4 wt% of the total weight of NBR and stannous chloride with a mass ratio of 0.2 wt% of the total weight of NBR are added for dynamic vulcanization of the blend. When the torque is stable, the TPV is taken out of the internal mixer and molded at 230° C. and 5 MPa to prepare a sheet with a thickness of about 2.0 mm, and a dumbbell-shaped specimen is cut out; Among them, the rubber is nitrile rubber (NBR) and the plastic is nylon 6 (PA6).
2. A method for recycling high-strength thermoplastic elastomer material, characterized in that: The method for preparing a high-toughness thermoplastic elastomer material according to claim 1, wherein the recycling process comprises the following steps: Step 1: Take the used high-strength and tough TPV with a heterogeneous network and zinc salt ionic bonds, and crush and melt the high-strength and tough TPV; Step 2: Then press it into tablets.
3. A method for recycling high-toughness thermoplastic elastomer material according to claim 2, characterized in that: The specific mechanical properties data and recycled data of high-strength and tough TPV are compared with those of ordinary TPV.