Oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material

By using an oxygen-rich high-entropy oxide/carbon fiber/piezoelectric modification layer composite anode material, the problems of volume expansion and slow transport of tin-based oxide anode materials in lithium-ion batteries are solved, thereby improving the cycle performance and conductivity of the battery.

CN117712308BActive Publication Date: 2026-11-17CHANGZHOU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311660103.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2026-11-17
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

Tin-based oxide anode materials for lithium-ion batteries suffer from large volume expansion and slow lithium-ion transport during cycling, leading to a decrease in battery specific capacity and cycle life.

Method used

An oxygen-rich high-entropy oxide/carbon fiber/piezoelectric modification layer composite anode material is adopted. By introducing porous carbon fiber and piezoelectric modification layer, the transport rate of lithium ions and electrons is improved and the material cracking problem caused by volume expansion is alleviated.

Benefits of technology

It improves the cycle performance and rate performance of lithium-ion batteries, enhances conductivity and interfacial lithium-ion transport capacity, and mitigates material damage caused by volume expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004589965450000111
    Figure BDA0004589965450000111
  • Figure HDA0004589965460000011
    Figure HDA0004589965460000011
  • Figure HDA0004589965460000012
    Figure HDA0004589965460000012
Patent Text Reader

Abstract

This invention belongs to the field of lithium-ion battery materials, specifically relating to an oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material. The oxygen-rich high-entropy oxide is prepared using a co-precipitation method, incorporating a highly conductive and inactive divalent element as one of the five principal components of the high-entropy oxide. This increases oxygen vacancies and improves conductivity, accelerating the transport rate of lithium ions and electrons. The porous carbon fiber is combined with the oxygen-rich high-entropy oxide to further improve the conductivity of the anode, alleviate volume expansion during cycling, improve cycle performance, and shorten the ion-electron transport distance, thereby enhancing the battery's rate performance. A functionalized piezoelectric modification layer is introduced, utilizing the mechanical stress generated by the alloying reaction to induce Bi... 0.5 Na 0.5 TiO3(BNT) generates a local electric field, realizing the conversion of mechanical energy into electrical energy, thereby improving the interfacial lithium-ion transport capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery materials, specifically relating to an oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material. Background Technology

[0002] Lithium-ion batteries, characterized by high energy density and high specific power, are key materials in the field of electrochemical energy storage. Tin-based oxides, as a new generation of lithium-ion battery anode materials, have attracted much attention due to their theoretical capacity being far higher than that of traditional graphite anodes. However, their continuous and significant volume expansion during cycling and slow lithium-ion transport and diffusion lead to a sharp decline in battery specific capacity and cycle life. The synergistic effect of composite oxide metal elements can overcome the intrinsic crystal structure defects of single-phase oxides, improve the diffusion kinetics of lithium ions in the crystal lattice, alleviate the kinetic imbalance between the anode and cathode, and achieve electrochemical activity and conductivity superior to single metal oxides.

[0003] High-entropy tin-based pyrochlore material system (A) 1 0.2 A 2 0.2 A 3 0.2 A 4 0.2 A 5 0.2 The theoretical specific capacity of 2Sn2O6 is 727 mAh / g, significantly higher than that of carbon materials, tin-based materials, and composite alloys, greatly expanding the design space for lithium-ion battery anode materials. Existing patents have prepared high-entropy tin-based pyrochlore materials using solid-state and hydrothermal methods (patent numbers: 202311135902.1, 202211617687.4), and obtained preliminary electrochemical performance at 200 mAh / g. -1 During charge-discharge cycles at current density, the highest initial discharge specific capacity can reach 964 mAh g. -1 However, after 100 cycles, the discharge specific capacity was 395 mAhg. -1 There is still a significant decline.

[0004] Carbon fiber (CF) is a novel high-strength, high-modulus fiber material with a carbon content of over 95%. Its excellent conductivity makes it widely used as a conductivity modifier in composite electrode materials. Patent CN104037393 A prepared a tin / graphene / carbon fiber composite lithium-ion battery anode material using ultrasonication, reduction, and drying methods; patent CN 105552312 A prepared a carbon fiber-coated lithium-ion battery anode sheet using spray coating; and patent CN104779378 A prepared a germanium-mesoporous carbon fiber composite lithium-ion battery anode material using electrospinning. These patents employed different methods to prepare carbon fiber composite materials. Combining with carbon materials helps alleviate problems such as material cracking and pulverization caused by uneven stress during lithium-ion extraction / insertion. Compared to the materials before combination, the electrochemical performance of the composite materials shows some improvement, but volume expansion remains an unresolved issue. Summary of the Invention

[0005] To address the problems identified in the background art, this invention provides an oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material. This material is formed by combining an oxygen-rich high-entropy oxide, porous carbon fiber, and a piezoelectric modification layer to create the composite anode material: (Y 0.2 La 0.2 Ce 0.2 Bi 0.2 M 0.2 )2Sn2O 6.4+2x / CF / Bi 0.5 Na 0.5 TiO3, where x is the valence of M; M = Ca, Mg, Al, Zn.

[0006] The preparation method of oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material includes the following steps:

[0007] (1) Weigh the corresponding nitrates or hydrochlorides according to the molar ratio of Y:La:Ce:Bi:M:Sn=1:1:1:1:1:5, then dissolve them in deionized water and stir magnetically at a speed of 400-600 r / min for 1-2 h. Add 20 wt% anhydrous ethanol as a dispersant and 0.1-2 g CTAB as a surfactant while stirring magnetically. The volume ratio of dispersant to deionized water is 1:4. Add diluted ammonia water with a concentration of 2 M and keep the pH of the solution at 9. After continuous stirring, carry out the precipitation reaction for 10 min and then centrifuge and filter to obtain the precipitate.

[0008] (2) Add n-pentanol to the precipitate and rotary evaporate it at a temperature of 80-95℃ to remove residual moisture and obtain dry powder. Place the obtained dry powder into an alumina crucible and calcine it in a muffle furnace at 800-1000℃ with a heating rate of 5-10℃ / min for 2-3 hours. After grinding, oxygen-enriched high-entropy oxide powder is obtained.

[0009] (3) The oxygen-enriched high-entropy oxide powder obtained in step (2) is mixed with carbon fiber at a mass ratio of (1.05-1):1 and placed in a ball mill jar with a ball-to-material ratio of (3-5):1. The rotation speed is 600-1200 r / min and the ball milling time is 2-5 h. The resulting mixture is taken out and placed in an argon atmosphere tube furnace for sintering at a temperature of 500-700℃ for 2-3 h. After natural cooling, the oxygen-enriched high-entropy oxide / carbon fiber composite electrode material is obtained.

[0010] (4) According to Bi 0.5 Na 0.5 The stoichiometric ratio of TiO3 (BNT) is determined by placing the oxides of the three elements into a ball mill jar for ball milling, drying after ball milling, and calcining at 800-1000℃ for 2-3 hours to obtain BNT for later use. The ball-to-material ratio is (3-5):1, the rotation speed is 300-600 r / min, and the ball milling time is 2-3 hours.

[0011] (5) The oxygen-enriched high-entropy oxide / carbon fiber material from step (3) and the BNT from step (4) are mixed at a ratio of 5-20% of the piezoelectric material to the composite electrode material. The mixture is then ball-milled in an inert atmosphere with a ball-to-material ratio of 3:1-6:1, a rotation speed of 300-600 r / min, and a ball-milling time of 8-12 h. The mixture is then calcined in air at 800-1000 °C for 1-2 h to obtain the oxygen-enriched high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material.

[0012] The application method of oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material includes the following steps:

[0013] (1) The materials were prepared according to the mass ratio of oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material: acetylene black: sodium carboxymethyl cellulose = 8:1:1;

[0014] (2) Add an appropriate amount of deionized water and grind and mix for 1 hour to obtain a uniform slurry. Coat the copper foil with the thickness controlled within 100-150 μm.

[0015] (3) After drying in a vacuum oven, the negative electrode sheet of the lithium battery is obtained by slicing. The lithium metal sheet is used as a reference electrode for the assembly of coin cells.

[0016] Compared with the prior art, the technical solution provided by this invention has the following advantages:

[0017] This invention uses high-conductivity elements such as Al or inactive divalent elements such as Zn, Ca, and Mg as one of the five principal components of high-entropy oxides. The substitution of low-valence elements can change the chemical formula of the oxide, increasing oxygen vacancies and improving conductivity, which is beneficial to accelerating the transport rate of lithium ions and electrons. Surfactants and dispersants are added during the preparation of powder, and powders with uniform distribution and small grain size are obtained through rapid co-precipitation reaction.

[0018] Combining porous carbon fibers with oxygen-rich high-entropy oxides can increase the conductivity of the negative electrode by introducing carbon. On the other hand, the hollow structure of the carbon fibers can help alleviate problems such as material cracking and pulverization caused by uneven stress during the lithium-ion extraction / insertion process, improve cycle performance, and shorten the transport distance between ions and electrons, thereby improving the rate performance of the battery.

[0019] This invention introduces a BNT-functionalized piezoelectric modification layer on the surface of a composite material. The mechanical stress generated by the alloying reaction induces the BNT to generate a local electric field, realizing the conversion of mechanical energy into electrical energy, thereby further improving the interfacial lithium-ion transport capacity and alleviating the volume expansion caused by the alloying reaction. Attached image description:

[0020] Figure 1 Example 1 (Y) 0.2 La 0.2 Ce 0.2 Bi 0.2 Ca 0.2 )2Sn2O 6.8 SEM image of / CF / BNT powder;

[0021] Figure 2 Example 1 (Y) 0.2 La 0.2 Ce 0.2 Bi 0.2 Ca 0.2 )2Sn2O 6.8 XRD pattern of the powder;

[0022] Figure 3 Example 2 (Y) 0.2 La 0.2 Ce 0.2 Bi 0.2 Ca 0.2 )2Sn2O 6.8 Cyclic capacity diagram of / CF / BNT powder;

[0023] Figure 4 Example 4 (Y) 0.2 La0.2 Ce 0.2 Bi 0.2 Mg 0.2 )2Sn2O 6.8 Cyclic capacity diagram of / CF / BNT powder. Detailed Implementation

[0024] The present invention will now be described in detail with reference to specific embodiments.

[0025] Example 1

[0026] (1) Yttrium nitrate, lanthanum nitrate, cerium nitrate, bismuth nitrate, calcium chloride, and tin chloride were prepared in a molar ratio of 1:1:1:1:1:5. Other reagents were weighed based on a yttrium nitrate mass of 1.6958 g. The weighed reagents were dissolved in 160 ml of deionized water. The solution was magnetically stirred at 500 r / min for 2 h. During stirring, 40 ml of 20 wt% anhydrous ethanol was added as a dispersant, and 1.9 g of CTAB was added as a surfactant. A 2 M ammonia solution was prepared using 25% ammonia water. The two solutions were then mixed, and the pH was maintained at 9 while the mixture was rapidly stirred. The reaction was allowed to proceed for 10 min to form a suspension. The suspension was then filtered and washed with deionized water and anhydrous ethanol to obtain the precipitate.

[0027] (2) Use 100ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95℃ to obtain dry powder. Calcinate the powder in a muffle furnace at 800℃ for 3h, then grind it to obtain oxygen-enriched high-entropy oxide powder.

[0028] (3) The oxygen-enriched high-entropy oxide powder from step (2) and carbon fiber (Jining Carbon Co., Ltd.) are placed in a ball mill jar at a mass ratio of 1:1. Ball milling beads are added at a ball-to-material mass ratio of 3:1, and anhydrous ethanol is added at a mass ratio of 2:1. The ball mill is started and milled at 800 r / min for 4 h. After drying, the mixture is placed in an argon atmosphere tube furnace for sintering at 600℃ for 3 h. After natural cooling, the oxygen-enriched high-entropy oxide / carbon fiber composite electrode material is obtained.

[0029] (4) According to the stoichiometric ratio of BNT, the oxides of the three elements were placed in a ball mill jar with a ball-to-material ratio of 4:1. After ball milling at 500 r / min for 2 h, the mixture was dried and calcined at 800 °C for 3 h to obtain BNT.

[0030] (5) The oxygen-enriched high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4) at a ratio of 10% of the piezoelectric material to the composite electrode material, and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h), and then calcined in air at 800 °C for 1 h to obtain the oxygen-enriched high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material.

[0031] The application methods of the above-mentioned oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite electrode material are as follows:

[0032] Weigh 0.1g of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material powder obtained in (5) above, 0.0125g of acetylene black, 0.625ml of sodium carboxymethyl cellulose solution with a mass fraction of 2% and 1ml of deionized water, mix and grind for 1h, then coat the slurry onto copper foil with a thickness of 100μm, and after vacuum drying, slice to obtain a negative electrode sheet. Use a lithium metal sheet as a reference electrode to assemble a coin cell.

[0033] Example 2

[0034] Step (1) is the same as in Example 1.

[0035] (2) Use 100ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95℃ to obtain dry powder. Calcinate the powder in a muffle furnace at 900℃ for 3h, then grind it to obtain oxygen-enriched high-entropy oxide powder.

[0036] Everything else is the same as in Example 1.

[0037] Example 3

[0038] Step (1) is the same as in Example 1.

[0039] (2) Use 100ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95℃ to obtain dry powder. The powder is then calcined in a muffle furnace at 1000℃ for 3 hours, and after grinding, oxygen-enriched high-entropy oxide powder is obtained.

[0040] Everything else is the same as in Example 1.

[0041] Example 4

[0042] (1) Yttrium nitrate, lanthanum nitrate, cerium nitrate, bismuth nitrate, magnesium chloride, and tin chloride were prepared in a molar ratio of 1:1:1:1:1:5. Other reagents were weighed based on a yttrium nitrate mass of 1.6872 g. The weighed reagents were dissolved in 160 ml of deionized water. The solution was magnetically stirred at 500 r / min for 2 h. During stirring, 40 ml of 20 wt% anhydrous ethanol was added as a dispersant, and 1.9 g of CTAB was added as a surfactant. A 2 M ammonia solution was prepared using 25% ammonia water. The two solutions were then mixed, and the pH was maintained at 9 while stirring rapidly. The mixture was allowed to react for 10 min to form a suspension. The suspension was then filtered and washed with deionized water and anhydrous ethanol to obtain the precipitate.

[0043] Everything else is the same as in Example 1.

[0044] Example 5

[0045] (1) Yttrium nitrate, lanthanum nitrate, cerium nitrate, bismuth nitrate, aluminum nitrate, and tin chloride were prepared in a molar ratio of 1:1:1:1:1:5. Other reagents were weighed based on a yttrium nitrate mass of 1.6958 g. The weighed reagents were dissolved in 160 ml of deionized water. The solution was magnetically stirred at 500 r / min for 2 h. During stirring, 40 ml of 20 wt% anhydrous ethanol was added as a dispersant, and 1.9 g of CTAB was added as a surfactant. A 2 M ammonia solution was prepared using 25% ammonia water. The two solutions were then mixed, and the pH was maintained at 9 while stirring rapidly. The mixture was allowed to react for 10 min to form a suspension. The suspension was then filtered and washed with deionized water and anhydrous ethanol to obtain the precipitate.

[0046] Everything else is the same as in Example 1.

[0047] Example 6

[0048] (1)-(2) Same as Example 1.

[0049] (3) The oxygen-enriched high-entropy oxide powder and carbon fiber from (2) above are placed in a ball mill jar at a mass ratio of 1.05:1. Ball milling beads are added at a ball-to-material mass ratio of 3:1, and ball milling media are added at a mass ratio of anhydrous ethanol to material of 2:1. The ball mill is started and ball milled at 800 r / min for 4 h. After stopping, the mixture is filtered and dried to obtain a mixture. The mixture is placed in an argon atmosphere tube furnace for sintering at a temperature of 600℃ for 3 h. After natural cooling, the oxygen-enriched high-entropy oxide / carbon fiber composite electrode material is obtained.

[0050] (4) According to the stoichiometric ratio of BNT, the oxides of the three elements were placed in a ball mill jar with a ball-to-material ratio of 4:1. After ball milling at 500 r / min for 2 h, the mixture was dried and calcined at 800 °C for 3 h to obtain BNT.

[0051] (5) Combine the oxygen-rich high-entropy oxide / carbon fiber composite electrode material obtained in (3) with the Bi obtained in (4). 0.5 Na 0.5 TiO3 was mixed with piezoelectric material accounting for 10% of the composite electrode material mass and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h). Then, it was calcined in air at 800 °C for 1 h to obtain an oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite electrode material.

[0052] The application methods of the above-mentioned oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite electrode material are as follows:

[0053] Weigh 0.1g of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material powder obtained in (5) above, 0.0125g of acetylene black, 0.625ml of sodium carboxymethyl cellulose solution with a mass fraction of 2% and 1ml of deionized water, mix and grind for 1h, then coat the slurry onto copper foil with a thickness of 100μm, and after vacuum drying, slice to obtain a negative electrode sheet. Use a lithium metal sheet as a reference electrode to assemble a coin cell.

[0054] Example 7

[0055] (1)-(4) Same as Example 1.

[0056] (5) The oxygen-enriched high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4) at a ratio of 15% of the piezoelectric material to the composite electrode material, and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h), and then calcined in air at 800 °C for 1 h to obtain the oxygen-enriched high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material.

[0057] The application methods of the above-mentioned oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite electrode material are as follows:

[0058] Weigh 0.1g of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material powder obtained in (5) above, 0.0125g of acetylene black, 0.625ml of sodium carboxymethyl cellulose solution with a mass fraction of 2% and 1ml of deionized water, mix and grind for 1h, then coat the slurry onto copper foil with a thickness of 100μm, and after vacuum drying, slice to obtain a negative electrode sheet. Use a lithium metal sheet as a reference electrode to assemble a coin cell.

[0059] Example 8

[0060] (1)-(4) are the same as in Example 1.

[0061] (5) The oxygen-enriched high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4) at a ratio of 5% of the piezoelectric material to the composite electrode material, and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h), and then calcined in air at 800 °C for 1 h to obtain the oxygen-enriched high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material.

[0062] The application method of the composite electrode material is the same as in Example 1.

[0063] Example 9

[0064] (1)-(4) Same as Example 1.

[0065] (5) The oxygen-enriched high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4) at a piezoelectric material content of 20% of the composite electrode material mass, and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h), and then calcined in air at 800 °C for 1 h to obtain the oxygen-enriched high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material.

[0066] The application method of the composite electrode material is the same as in Example 1.

[0067] Comparative Example 1

[0068] (1) Prepare a mixture of yttrium nitrate, lanthanum nitrate, cerium nitrate, bismuth nitrate, neodymium nitrate, and tin chloride in a molar ratio of 1:1:1:1:1:5. Weigh the other reagents based on a mass of 1.7345 g of yttrium nitrate. Dissolve the weighed reagents in 160 ml of deionized water. Stir the solution magnetically at 500 r / min for 2 h. During stirring, add 40 ml of 20 wt% anhydrous ethanol as a dispersant and 1.9 g of CTAB as a surfactant. Prepare a 2 M ammonia solution with a mass fraction of 25-28%. Mix the two solutions while maintaining the pH at 9 and stirring rapidly. React for 10 min to form a suspension. Then, filter the suspension using deionized water and anhydrous ethanol to obtain the precipitate.

[0069] (2) Use 100 ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95°C to obtain dry powder. Calcinate the powder in a muffle furnace at 800°C for 3 h, then grind it to obtain high-entropy oxide powder.

[0070] (3) The high-entropy oxide powder and carbon fiber from (2) above are placed in a ball mill jar at a mass ratio of 1:1. Ball milling beads are added at a ball-to-material mass ratio of 3:1, and ball milling media are added at a mass ratio of anhydrous ethanol to material of 2:1. The ball mill is started and ball milled at 800 r / min for 4 h. After stopping, the mixture is filtered and dried to obtain a mixture. The mixture is placed in an argon atmosphere tube furnace for sintering at a temperature of 600℃ for 3 h. After natural cooling, the high-entropy oxide / carbon fiber composite electrode material is obtained.

[0071] (4) According to the stoichiometric ratio of BNT, the oxides of the three elements were placed in a ball mill jar with a ball-to-material ratio of 4:1. After ball milling at 500 r / min for 2 h, the mixture was dried and calcined at 800 °C for 3 h to obtain BNT.

[0072] (5) The high-entropy oxide / carbon fiber composite electrode material obtained in (3) and the BNT obtained in (4) are mixed at a ratio of 10% of the piezoelectric material to the composite electrode material and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h). Then, the high-entropy oxide / carbon fiber / piezoelectric modified layer composite electrode material is obtained by calcining in air at 800 °C for 1 h.

[0073] The application method of the composite electrode material is the same as in Example 1.

[0074] Comparative Example 2

[0075] Step (1) is the same as in Example 1.

[0076] (2) Use 100ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95℃ to obtain dry powder. Calcinate the powder in a muffle furnace at 800℃ for 3h, then grind it to obtain oxygen-enriched high-entropy oxide powder.

[0077] (3) The oxygen-enriched high-entropy oxide powder and carbon fiber from (2) above are placed in a ball mill jar at a mass ratio of 1:1. Ball milling beads are added at a ball-to-material mass ratio of 3:1, and ball milling media are added at a mass ratio of anhydrous ethanol to material of 2:1. After ball milling at 800 r / min for 4 h, the mixture is filtered and dried to obtain a mixture. The mixture is then placed in an argon atmosphere tube furnace for sintering at a temperature of 600℃ for 3 h. After natural cooling, the oxygen-enriched high-entropy oxide / carbon fiber composite electrode material is obtained.

[0078] The application method of the composite electrode material is the same as in Example 1.

[0079] Comparative Example 3

[0080] Step (1) is the same as in Example 1.

[0081] (2) Use 100ml of n-pentanol as a solvent to remove moisture from the precipitate by rotary evaporation at a temperature of 95℃ to obtain dry powder. Calcinate the powder in a muffle furnace at 800℃ for 3h, then grind it to obtain oxygen-enriched high-entropy oxide powder.

[0082] (3) According to the stoichiometric ratio of BNT, the oxides of the three elements were placed in a ball mill jar with a ball-to-material ratio of 4:1. After ball milling at 500 r / min for 2 h, the mixture was dried and calcined at 800 °C for 3 h to obtain BNT.

[0083] (4) The oxygen-enriched high-entropy oxide negative electrode material obtained in (2) and the BNT obtained in (3) are mixed at a piezoelectric material content of 10% of the composite electrode material and ball-milled in an inert atmosphere (ball-to-material ratio of 3:1, rotation speed of 300 r / min, ball-milling time of 12 h); and calcined in air at 800 °C for 1 h to obtain the oxygen-enriched high-entropy oxide / piezoelectric modified layer composite electrode material.

[0084] The application method of the composite electrode material is the same as in Example 1.

[0085] The lithium batteries prepared in Examples 1-6 and Comparative Examples 1-3 were subjected to charge-discharge experiments on the Newway Battery Testing System using the constant current charge-discharge test standard. The results are as follows:

[0086] Table 1 Discharge capacity and coulombic efficiency

[0087]

[0088] The described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A composite anode material of oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer, characterized in that, The composite anode material is a composite anode material formed by combining oxygen-rich high-entropy oxide, porous carbon fiber, and piezoelectric modification layer. The structural formula of the oxygen-rich high-entropy oxide is as follows: (Y 0.2 La 0.2 Ce 0.2 Bi 0.2 M 0.2 )2Sn2O 6.4+2x x is the valence of M; M = Ca, Mg, Al, Zn; The preparation steps of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modified layer composite anode material are as follows: (1) According to (Y) 0.2 La 0.2 Ce 0.2 Bi 0.2 M 0.2 )2Sn2O 6.4+2x According to the stoichiometric ratio, the nitrate or chloride raw materials of the above elements are dissolved in deionized water, anhydrous ethanol, CTAB and diluted ammonia solution are added, the pH is kept at 9, and the mixture is stirred continuously to obtain a precipitate, which is then filtered to obtain the precipitate. (2) Add n-pentanol to the precipitate and rotary evaporate to remove residual water to obtain dry powder, and calcine in air to obtain oxygen-enriched high-entropy oxide powder. (3) The powder in step (2) is mixed with carbon fiber and ball-milled and dried to obtain a mixture. The mixture is placed in an argon atmosphere tube furnace for sintering and naturally cooled to obtain an oxygen-rich high-entropy oxide / carbon fiber composite electrode material. (4) According to Bi 0.5 Na 0.5 The stoichiometric ratio of TiO3 was determined by placing the oxides of the three elements into a ball mill jar for wet ball milling, followed by drying and calcination to obtain BNT for later use. (5) The oxygen-rich high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4), ball-milled, and calcined to obtain the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite negative electrode material.

2. A method for preparing the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 1, characterized in that, The preparation method steps are as follows: (1) According to (Y) 0.2 La 0.2 Ce 0.2 Bi 0.2 M 0.2 )2Sn2O 6.4+2x According to the stoichiometric ratio, the nitrate or chloride raw materials of the above elements are dissolved in deionized water, anhydrous ethanol, CTAB and diluted ammonia solution are added, the pH is kept at 9, and the mixture is stirred continuously to obtain a precipitate, which is then filtered to obtain the precipitate. (2) Add n-pentanol to the precipitate and rotary evaporate to remove residual water to obtain dry powder, and calcine in air to obtain oxygen-enriched high-entropy oxide powder. (3) The powder in step (2) is mixed with carbon fiber and ball-milled and dried to obtain a mixture. The mixture is placed in an argon atmosphere tube furnace for sintering and naturally cooled to obtain an oxygen-rich high-entropy oxide / carbon fiber composite electrode material. (4) According to Bi 0.5 Na 0.5 The stoichiometric ratio of TiO3 was determined by placing the oxides of the three elements into a ball mill jar for wet ball milling, followed by drying and calcination to obtain BNT for later use. (5) The oxygen-rich high-entropy oxide / carbon fiber composite electrode material obtained in step (3) is mixed with the BNT obtained in step (4), ball-milled, and calcined to obtain the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite negative electrode material.

3. The preparation method of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 2, characterized in that, In step (1), the raw materials are prepared according to the molar ratio of elemental composition Y:La:Ce:Bi:M:Sn=1:1:1:1:1:5; the stirring speed is 400-600r / min, the stirring time is 1-2h, the volume ratio of anhydrous ethanol to deionized water is 1:4, the amount of CTAB added is 0.1-2g, and the concentration of diluted ammonia water is 2M.

4. The preparation method of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 2, characterized in that, In step (2), the rotary evaporation temperature is 80-95℃, the calcination temperature is 800-1000℃, the heating rate is 5-10℃ / min, and the calcination time is 2-3h.

5. The preparation method of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 2, characterized in that, In step (3), the mass ratio of powder to carbon fiber is (1-1.05):1, the ball-to-material ratio is (3-5):1, the rotation speed is 600-1200 r / min, the ball milling time is 2-5 h, the sintering temperature is 500-700 ℃, and the sintering time is 2-3 h.

6. The preparation method of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 2, characterized in that, In step (4), the ball-to-material ratio is (3-5):1, the rotation speed is 300-600 r / min, the ball milling time is 2-6 h, the calcination temperature is 800-1000 ℃, and the calcination time is 2-3 h.

7. The preparation method of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 2, characterized in that, Step (5) requires ball milling in an inert atmosphere. The piezoelectric material accounts for 5-20% of the mass of the composite electrode material. The ball-to-material ratio is (3-6):

1. The rotation speed is 300-600 r / min. The ball milling time is 8-12 h. The calcination temperature is 800-1000 ℃. The calcination time is 1-2 h.

8. An application of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 1, characterized in that, The composite anode material is used to prepare lithium-ion battery anode sheets.

9. The application of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 8, characterized in that, The method for preparing the electrode sheet is as follows: the composite negative electrode material is mixed with acetylene black, binder and deionized water in a mass ratio of 8:1:1, ground for 1 hour, and the resulting slurry is coated on copper foil and then vacuum dried to prepare a lithium-ion battery negative electrode sheet.

10. The application of the oxygen-rich high-entropy oxide / carbon fiber / piezoelectric modification layer composite anode material according to claim 8, characterized in that, The binder is a pre-prepared aqueous solution of sodium carboxymethyl cellulose with a concentration of 2 wt%; the slurry applied to the copper foil has a thickness of 100-150 μm.

Citation Information

Patent Citations

  • Preparation method for tin / graphene / carbon fiber composite lithium battery cathode material

    CN104037393A

  • Preparation method of cathode material of germanium-mesoporous carbon fiber composite lithium battery

    CN104779378A

  • Preparation method of carbon-fiber-coated lithium battery negative electrode plate

    CN105552312A

  • Preparation method of zinc-nitrate battery based on high-entropy oxide

    CN117026257A

  • High-entropy pyrochlore structure oxide battery negative electrode material with oxygen separation caused by B-site low-valence doping and preparation method of high-entropy pyrochlore structure oxide battery negative electrode material

    CN117038922A