Modified silica composite gel electrolyte, its preparation method and application
By modifying silica and mixing it with polymer monomers, a uniformly dispersed composite gel electrolyte was prepared, which solved the problems of insufficient ionic conductivity and mechanical properties of gel polymer electrolytes, and improved the safety and electrochemical performance of solid-state batteries.
Patent Information
- Application Number
- CN202311726666.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Existing gel polymer electrolytes have shortcomings in terms of ionic conductivity and mechanical properties. In particular, the ionic conductivity of high-polymer gel electrolytes is limited, and the uneven dispersion of inorganic fillers in the polymer matrix affects battery performance.
A green and environmentally friendly method was used to modify silica. Through the synergistic effect of plant polyphenols, metal salts and buffers, a uniformly dispersed modified silica was formed. This modified silica was then mixed with polymer monomers, lithium salts and initiators to carry out an in-situ polymerization reaction to prepare a composite gel electrolyte.
The composite gel electrolyte improves the ionic conductivity and mechanical properties, enhances the safety and electrochemical performance of solid-state batteries, and achieves uniform dispersion and efficient lithium-ion migration.
Smart Images

Figure CN117712464B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a modified silica composite gel electrolyte, its preparation method, and its application. Background Technology
[0002] With the expansion of markets such as consumer electronics, electric vehicles, and energy storage, batteries using liquid organic electrolytes are increasingly unable to meet the demands in terms of safety and energy density. Solid electrolytes are the core component of solid-state batteries, mainly divided into inorganic solid electrolytes (including oxide electrolytes and sulfide electrolytes) and solid polymer electrolytes. While inorganic solid electrolytes possess high ionic conductivity, their inherent brittleness increases processing difficulty, and their high interfacial resistance limits their practical applications. Solid polymer electrolytes, although possessing a certain degree of toughness and ease of processing, suffer from poor electrochemical stability and low ionic conductivity and transport number. In contrast, gel electrolytes, composed of a polymer matrix and a liquid electrolyte, are attracting increasing research attention. Gel polymer electrolytes offer a higher potential window and better mechanical strength than liquid electrolytes, and can provide higher ionic conductivity than all-solid-state electrolytes. Furthermore, the liquid electrolyte component in gel polymer electrolytes is confined within the polymer matrix, effectively reducing the risk of electrolyte leakage and enhancing battery safety.
[0003] Currently, conventional methods for preparing gel polymer electrolytes mainly fall into two categories: (1) first, a porous polymer film is prepared, and then an electrolyte is added during battery assembly to achieve gelation. (2) Precursor polymer monomers and initiators are added to the liquid electrolyte, and in-situ polymerization and gelation are achieved after electrolyte injection. The in-situ gelation route is compatible with the current industrialized electrolyte injection and formation processes, and has lower battery impedance, thus showing greater development potential. In gel electrolytes formed by in-situ polymerization, the degree of polymerization is one of the important factors affecting the physicochemical properties of gel electrolytes. Low-polymer gel electrolytes have poor thermal stability and mechanical properties, and may be penetrated by lithium dendrites and develop cracks during battery cycling, leading to battery performance degradation or even failure. Therefore, the synthesis of high-polymer gel electrolytes is crucial for developing batteries with high stability and high safety, but high-polymer gel electrolytes face the challenge of limited ionic conductivity.
[0004] Compared to pure gel electrolytes, composite gel electrolytes prepared by adding inorganic fillers can provide additional lithium-ion transport sites and pathways, further improving ionic conductivity and thus accelerating lithium-ion reaction kinetics. Although introducing inorganic fillers into the polymer network can address the problems of poor ionic conductivity and weak mechanical properties of gel electrolytes, the inherently high specific surface energy and poor compatibility of inorganic fillers with the polymer matrix may lead to uneven dispersion within the polymer matrix, resulting in uneven lithium-ion flux in the composite electrolyte system and consequently affecting the electrochemical performance of the battery.
[0005] Silica is a commonly used inorganic filler in composite gel electrolytes. CN03119735 discloses a composite solid polymer electrolyte prepared from a polymer matrix, lithium salt, and modified inorganic nanoparticles, wherein the surface groups of the silica nanoparticles are hydroxyl, trimethylsilyl, and polydimethylsilane; CN201810072837.5 discloses a composite gel polymer electrolyte membrane using ionic liquid-modified nano-silica as filler; CN111416146B discloses silica nanoparticles with pyromellitic acid diimide bridges synthesized by amidation reaction and their application in composite solid polymer electrolytes; CN115588773A discloses modified silica, a solid electrolyte, and a lithium-ion battery, wherein the modified silica is rich in alkylamine groups. Although surface modification of silica with amides or silanes can improve its dispersibility, most modification methods face problems such as expensive and toxic raw materials, complex synthesis processes, and serious pollution and energy consumption during synthesis. Summary of the Invention
[0006] To address the problems of existing technologies, this invention first modifies silica in a green, environmentally friendly, simple, and controllable manner, and then adds the modified silica as an inorganic filler to the composite gel electrolyte. This has significant advantages in improving the ionic conductivity and mechanical properties of the gel electrolyte, resulting in a significant improvement in the safety and electrochemical performance of solid-state batteries.
[0007] This invention first provides a method for preparing a modified silica composite gel electrolyte, which includes the following steps:
[0008] A. Dissolve plant polyphenols in deionized water to obtain a polyphenol solution; dissolve metal salts in deionized water to obtain a metal salt solution; dissolve a buffer in deionized water to obtain a buffer solution.
[0009] B. Mix the polyphenol solution obtained in step A with the buffer solution, add silica, and sonicate evenly at room temperature. Then add the metal salt solution obtained in step A, stir and react at room temperature, and then centrifuge, wash and vacuum dry to obtain modified silica.
[0010] C. Mix the modified silica, polymer monomer, lithium salt, initiator and organic solvent obtained in step B evenly to obtain a composite gel electrolyte precursor solution.
[0011] D. The composite gel electrolyte precursor solution obtained in step C is subjected to in-situ polymerization to obtain modified silica composite gel electrolyte.
[0012] In the above preparation method, in step A, the plant polyphenols are selected from at least one of tannic acid, ellagic acid, catechin, or gallic acid.
[0013] In the above preparation method, in step A, the mass concentration of the polyphenol solution is 1-5 mg / mL.
[0014] In the above preparation method, in step A, the metal ions in the metal salt are selected from Fe. 3+ Mn 2+ Al 3+ or Zn 2+ At least one of them, wherein the anion is selected from Cl. - NO3 - or SO4 2- At least one of them.
[0015] Preferably, in the above preparation method, in step A, the metal salt is selected from ferric chloride, ferric sulfate, manganese sulfate, zinc sulfate, zinc chloride, or aluminum chloride.
[0016] In the above preparation method, in step A, the mass concentration of the metal salt solution is 1-5 mg / mL.
[0017] In the above preparation method, in step A, the buffer is selected from at least one of tris(hydroxymethyl)aminomethane, tris(hydroxymethyl)aminomethane hydrochloride, bis(2-hydroxyethylamino)tris(hydroxymethyl)methane, or bis(2-hydroxyethylamino)tris(hydroxymethyl)methane hydrochloride.
[0018] In the above preparation method, in step A, the mass concentration of the buffer solution is 0.1–0.5 mg / mL.
[0019] In the above preparation method, in step B, the molar ratio of polyphenols in the polyphenol solution to metal salts in the metal salt solution is 1:20-40, the amount of buffer solution added is used to control the pH value of the system to 3-6, and the mass concentration of silica in the system is 1-10 mg / mL.
[0020] In the above preparation method, in step B, the silicon dioxide has a size of micro-nano scale.
[0021] In the above preparation method, in step B, the time for ultrasonic dispersion to achieve uniformity is 30-60 minutes.
[0022] In the above preparation method, in step B, the stirring reaction time is 6 to 36 hours.
[0023] Preferably, in the above preparation method, the stirring reaction time in step B is 10-14 hours.
[0024] In the above preparation method, in step B, the stirring speed is 300-500 r / min.
[0025] In the above preparation method, in step B, the temperature of vacuum drying is 50-70℃.
[0026] In the above preparation method, in step B, the vacuum drying time is 8 to 16 hours.
[0027] In the above preparation method, in step C, the polymer monomer is a multifunctional acrylate monomer selected from at least one of pentaerythritol tetraacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, bis(trimethylolpropane)tetraacrylate, or trimethylolpropane triacrylate.
[0028] In the above preparation method, in step C, the initiator is an azo compound selected from at least one of azobisisobutyronitrile, dimethyl azobisisobutyrate, or azobisisoheptanenitrile.
[0029] In the above preparation method, in step C, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide.
[0030] In the above preparation method, in step C, the organic solvent is selected from at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, fluoroethylene carbonate, methyl butyrate, ethyl butyrate, or ethyl acetate.
[0031] Preferably, in the above preparation method, in step C, the organic solvent is a mixed solvent of ethylene carbonate, methyl ethyl carbonate and diethyl carbonate in a volume ratio of 1:1:1.
[0032] In the above preparation method, in step C, the mass percentage of the polymer monomer in the composite gel electrolyte precursor solution is 3-8%.
[0033] In the above preparation method, in step C, the initiator has a mass percentage content of 0.1% to 0.5% in the composite gel electrolyte precursor solution.
[0034] In the above preparation method, in step C, the concentration of the lithium salt in the composite gel electrolyte precursor solution is 0.8–1.2 mol / L.
[0035] In the above preparation method, in step C, the mass percentage of the modified silica in the composite gel electrolyte precursor solution is 0.01-5%.
[0036] In the above preparation method, in step D, the temperature of the in-situ polymerization reaction is 50–80°C.
[0037] In the above preparation method, in step D, the in-situ polymerization reaction takes 10–72 h.
[0038] The present invention also provides a modified silica composite gel electrolyte, which is prepared by the above method.
[0039] The present invention also provides the application of the above-mentioned modified silica composite gel electrolyte in in-situ gelled solid-state batteries.
[0040] Based on the above-mentioned modified silica composite gel electrolyte (composite gel electrolyte precursor solution), the present invention also provides an in-situ gelled solid-state battery, the preparation method of which includes the following steps:
[0041] The positive electrode, separator, and negative electrode are assembled into a battery using conventional methods in the art. Then, the composite gel electrolyte precursor solution obtained in step C of the above-mentioned method for preparing modified silica composite gel electrolyte is injected, and then the battery is sealed. Finally, it undergoes an in-situ polymerization reaction to obtain the final product.
[0042] The beneficial effects of this invention are:
[0043] This invention modifies silica using polyphenols, metal salts, and buffers. The raw material, plant polyphenols, is widely distributed in nature and is an important class of phytochemicals. Polyphenols can crosslink with various metal ions to form complexes with different coordination numbers under controlled pH and reaction time. These polyphenol-metal ion complexes possess advantages such as strong adhesion, low cost, good usability, and structural diversity. The modified silica has uniformly distributed hydroxyl groups and Lewis acid sites. In the composite gel electrolyte formed by in-situ polymerization, this modified silica, as an inorganic filler component, not only disperses uniformly in the polymer network and forms bonds with it to enhance mechanical properties, but also provides abundant lithium-ion migration sites, improving ion transport rates.
[0044] The synthesis process of the composite gel electrolyte of this invention is green, environmentally friendly, and pollution-free, and is simple and controllable; solid-state batteries using the above-mentioned composite gel electrolyte show significant improvements in safety and electrochemical performance. Attached Figure Description
[0045] Figure 1 This is an SEM image of the modified inorganic filler from Example 1.
[0046] Figure 2 Optical photographs of the composite gel electrolytes in Example 1 and Comparative Examples 1-2.
[0047] Figure 3 The graph shows a comparison of the cycle performance of Examples 1-3 and Comparative Examples 1-2.
[0048] Figure 4 The graph shows a comparison of the rate performance of Examples 1-3 and Comparative Examples 1-2.
[0049] Figure 5 This is a diagram illustrating the safety performance of a solid-state battery in Example 1. Detailed Implementation
[0050] Specifically, a method for preparing a modified silica composite gel electrolyte includes the following steps:
[0051] A. Dissolve plant polyphenols in deionized water to obtain a polyphenol solution; dissolve metal salts in deionized water to obtain a metal salt solution; dissolve a buffer in deionized water to obtain a buffer solution.
[0052] B. Mix the polyphenol solution obtained in step A with the buffer solution, add silica, and ultrasonically disperse it evenly at room temperature (at this time, a polyphenol-silica dispersion is obtained). Then add the metal salt solution obtained in step A, stir the reaction at room temperature, and then centrifuge, wash and vacuum dry to obtain modified silica.
[0053] C. Mix the modified silica, polymer monomer, lithium salt, initiator and organic solvent obtained in step B evenly to obtain a composite gel electrolyte precursor solution.
[0054] D. The composite gel electrolyte precursor solution obtained in step C is subjected to in-situ polymerization to obtain modified silica composite gel electrolyte.
[0055] The inventors discovered that polyphenols possess multiple hydroxyl groups, and adjacent hydroxyl groups can form complexes with metal ions through coordination. These complexes can adhere well to the surface of silica nanoparticles, altering the surface properties of silica. The concentrations of the polyphenol solution, the metal salt solution, and the reaction time affect the degree of silica modification, thereby influencing the ionic conductivity and mechanical properties of the subsequent composite gel electrolyte. Experiments showed that in step A of this invention, the mass concentrations of the polyphenol solution and the metal salt solution are controlled to be 1–5 mg / mL.
[0056] In step A of this invention, the plant polyphenol is selected from at least one of tannic acid, ellagic acid, catechin, or gallic acid. The metal ion in the metal salt is selected from Fe. 3+ Mn 2+ Al 3+ or Zn 2+ At least one of the following, wherein the anion is selected from Cl-, NO3-, etc. - or SO4 2- At least one of the following: preferably ferric chloride, ferric sulfate, manganese sulfate, zinc sulfate, zinc chloride, or aluminum chloride.
[0057] In this invention, the buffer is used to regulate the pH of the solution. The pH of the solution affects the number of polyphenols that coordinate with metal ions. The pH of the solution is regulated by controlling the concentration and amount of buffer added. Therefore, in step A of this invention, the mass concentration of the buffer is controlled to be 0.1-0.5 mg / mL. The buffer is selected from at least one of tris(hydroxymethyl)aminomethane, tris(hydroxymethyl)aminomethane hydrochloride, bis(2-hydroxyethylamino)tris(hydroxymethyl)methane, or bis(2-hydroxyethylamino)tris(hydroxymethyl)methane hydrochloride.
[0058] As described above, this invention requires controlling the degree of silica modification to obtain modified silica suitable for composite gel electrolytes. Through experimentation, in step B of this invention, the molar ratio of polyphenols in the polyphenol solution to metal salts in the metal salt solution is 1:20–40, the amount of buffer solution added is used to control the pH of the system to 3–6, and the mass concentration of silica in the system is 1–10 mg / mL. Here, "system" refers to the solution system after the addition of the metal salt solution.
[0059] In step B of this invention, the silicon dioxide has a size of micro-nano scale.
[0060] In step B of this invention, the time for ultrasonic dispersion to achieve uniformity is 30–60 min.
[0061] Experiments have shown that, with a fixed reactant concentration, different reaction times result in different degrees of silica modification, which in turn affect the ionic conductivity and mechanical properties of the subsequent composite gel electrolyte. Therefore, in step B of this invention, the stirring reaction time is controlled to be 6–36 h. When the stirring reaction time is controlled to be 10–14 h, the performance can be further improved.
[0062] In step B of this invention, the stirring speed is 300-500 r / min.
[0063] In step B of this invention, the temperature of the vacuum drying is 50–70°C.
[0064] In step B of this invention, the vacuum drying time is 8 to 16 hours.
[0065] In step C of this invention, the polymer monomer is a multifunctional acrylate monomer, selected from at least one of pentaerythritol tetraacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, di(trimethylolpropane) tetraacrylate, or trimethylolpropane triacrylate; the initiator is an azo compound, selected from azobisisobutyronitrile, dimethyl azobisisobutyrate, or azobisisoheptanenitrile. At least one of the following: the lithium salt is selected from lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluorooxalato)borate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide; the organic solvent is selected from at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, fluoroethylene carbonate, methyl butyrate, ethyl butyrate, or ethyl acetate; preferably a mixture of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate in a volume ratio of 1:1:1.
[0066] The amount of modified silica used affects the degree of polymerization of the composite gel electrolyte, further affecting its stability, mechanical properties, and ionic conductivity. Experiments have shown that in step C of this invention, the polymer monomer content in the composite gel electrolyte precursor solution is 3-8% by mass; the initiator content is 0.1-0.5% by mass; the lithium salt concentration is 0.8-1.2 mol / L; and the modified silica content is 0.01-5% by mass.
[0067] To directly obtain the modified silica composite gel electrolyte, in step D of this invention, the temperature of the in-situ polymerization reaction is controlled at 50–80°C, and the time of the in-situ polymerization reaction is controlled at 10–72 h.
[0068] The present invention also provides a modified silica composite gel electrolyte, which is prepared by the above method.
[0069] The present invention also provides the application of the above-mentioned modified silica composite gel electrolyte in in-situ gelled solid-state batteries.
[0070] Based on the above-mentioned modified silica composite gel electrolyte (composite gel electrolyte precursor solution), the present invention also provides an in-situ gelled solid-state battery, the preparation method of which includes the following steps:
[0071] The positive electrode, separator, and negative electrode are assembled into a battery using conventional methods in the art. Then, the composite gel electrolyte precursor solution obtained in step C of the above-mentioned method for preparing modified silica composite gel electrolyte is injected, and then the battery is sealed. Finally, it undergoes an in-situ polymerization reaction to obtain the final product.
[0072] The present invention will be further described in detail below through embodiments, but the scope of protection of the present invention is not limited to the embodiments described herein.
[0073] Example 1
[0074] The specific preparation method of the modified silica, gel composite electrolyte, and in-situ gelled solid-state battery in this embodiment is as follows:
[0075] (1) Preparation of modified silica: 0.1 g tannic acid was added to 50 mL deionized water and stirred at room temperature to dissolve to obtain a polyphenol solution; 0.2 g zinc chloride was added to 50 mL deionized water and stirred at room temperature to dissolve to obtain a metal salt solution; 0.5 mg tris(hydroxymethyl)aminomethane hydrochloride was added to 5 mL deionized water and stirred at room temperature to dissolve to obtain a buffer solution.
[0076] (2) Mix the polyphenol solution with the buffer solution, add 0.5g of nano silica, and sonicate for 30min at room temperature; then add the metal salt solution and magnetically stir for 12h at room temperature; finally, centrifuge and wash the mixed solution, and vacuum dry at 60℃ for 12h to obtain modified silica.
[0077] (3) Preparation of gel composite electrolyte precursor solution: Based on the total mass of the precursor solution being 100%, lithium hexafluorophosphate, organic solvents (ethylene carbonate, methyl ethyl carbonate and diethyl carbonate), polymer monomer pentaerythritol tetraacrylate, thermal initiator azobisisobutyronitrile, and modified silica were mixed in proportion to obtain the precursor solution; wherein the concentration of lithium hexafluorophosphate was 1.0 mol / L, the volume ratio of organic solvents ethylene carbonate, methyl ethyl carbonate and diethyl carbonate was 1:1:1, and the mass percentages of pentaerythritol tetraacrylate, azobisisobutyronitrile and modified silica were 5%, 0.2% and 0.05%, respectively.
[0078] (4) In-situ gelation assembly of coin cells: The positive electrode material (NCM811), conductive agent (acetylene black), and binder (PVDF) are mixed evenly at a mass ratio of 95:3:2, and then dispersed in an N-methylpyrrolidone solution and stirred evenly. The prepared slurry is evenly coated on aluminum foil and then dried to obtain the positive electrode sheet. The prepared positive electrode sheet-separator-negative electrode are assembled into a battery using traditional processes, and then the electrolyte precursor is injected and sealed. The assembled battery is left to stand at 60°C for 12 hours and then undergoes an in-situ polymerization reaction to obtain the in-situ gelated solid battery (the composite gel electrolyte precursor solution is left to stand at 60°C for 12 hours and then undergoes an in-situ polymerization reaction to obtain the composite gel electrolyte).
[0079] Figure 1 This is a SEM image of the modified silica in Example 1 of the present invention. Figure 1 It can be seen that the modified silica prepared in this embodiment consists of spherical particles with a particle size of about 300 nm.
[0080] Figure 2 These are optical photographs of the composite gel electrolytes in Example 1 and Comparative Examples 1-2 of the present invention. Figure 2 It can be seen that the composite gel electrolyte in Example 1 is a complete gel polymer without liquid flow; while the gel electrolyte in Comparative Example 1 shows cracking, and the composite gel electrolyte in Comparative Example 2 shows delamination. This indicates that the modified silica provided by the present invention can effectively achieve uniform dispersion and interfacial compatibility in the polymer network, while improving the mechanical properties of the gel electrolyte.
[0081] Example 2
[0082] The preparation methods of the modified silica, gel composite electrolyte and in-situ gelled solid battery in this embodiment are basically the same as those in Example 1. The only difference is that the magnetic stirring time at room temperature in step (2) is 6 hours.
[0083] Example 3
[0084] The preparation methods of the modified silica, gel composite electrolyte and in-situ gelled solid battery in this embodiment are basically the same as those in Example 1. The only difference is that the magnetic stirring time at room temperature in step (2) is 18h.
[0085] Comparative Example 1
[0086] This comparative example provides a method for preparing a gel electrolyte and an in-situ gelled solid-state battery. The difference from Example 1 is that no inorganic filler is added in the preparation of the gel electrolyte precursor solution.
[0087] Comparative Example 2
[0088] This comparative example provides a method for preparing a composite gel electrolyte and an in-situ gelled solid-state battery. The difference from Example 1 is that unmodified silica is directly added as an inorganic filler in the preparation of the gel electrolyte precursor solution.
[0089] Experimental Example 1
[0090] The lithium-ion room temperature conductivity of the composite gel electrolytes in Examples 1-3 and Comparative Examples 1-2 was measured, and the results are shown in Table 1.
[0091] Lithium-ion room temperature conductivity testing: The gel electrolyte precursor solutions of the examples and comparative examples were dropped between two stainless steel sheets to assemble a coin cell; the assembled cells were placed at 60°C for 10 hours and then subjected to in-situ polymerization; then EIS testing was performed using an electrochemical workstation with a frequency range of 0.1–10. 6 The ionic conductivity is calculated using the formula σ = L / (R × S) at a frequency of Hz and an amplitude of 10mV, where σ is the ionic conductivity (S / cm), L is the thickness of the solid electrolyte membrane (cm), R is the resistance of the solid electrolyte membrane (Ω), and S is the effective membrane area (cm²). 2 ).
[0092] Table 1. Test results of lithium-ion conductivity and electrochemical performance of the examples and comparative examples.
[0093] name Ionic conductivity (mS / cm) Capacity retention rate (%) Rate performance (1C: mAh / g) Example 1 0.802 97.45 104.02 Example 2 0.796 87.17 91.78 Example 3 0.653 94.02 78.42 Comparative Example 1 0.326 90.48 42.44 Comparative Example 2 0.158 76.72 58.90
[0094] Experimental Example 2
[0095] The capacity retention of the in-situ gelled solid-state batteries of Examples 1-3 and Comparative Examples 1-2 was tested, and the results are shown in Table 1 and 2. Figure 3 .
[0096] The testing conditions were as follows: the battery was charged at a constant current rate of 0.5C at 25°C until the voltage reached 4.25V, and then discharged at a constant current rate of 0.5C until the voltage reached 3V. The battery underwent 100 charge and discharge cycles according to this charge and discharge regime. The cycle retention rate after 100 cycles was calculated using the following formula: Cycle retention rate (%) = (Discharge capacity at the 100th cycle / Discharge capacity at the 1st cycle) × 100%.
[0097] Experimental Example 3
[0098] The in-situ gelled solid-state batteries of Examples 1-3 and Comparative Examples 1-2 were tested for charge-discharge rate performance at 0.1C, 0.2C, 0.5C, and 1C. The results are shown in Table 1 and 2. Figure 4 .
[0099] As shown in Table 1, compared to the comparative examples, the composite gel electrolyte containing modified silica provided by this invention has higher ion transport number and ionic conductivity. Solid-state batteries obtained using this electrolyte exhibit excellent cycle performance and rate performance. Specifically, the composite gel electrolytes in Examples 1-3 have an ionic conductivity of 0.6-0.8 mS / cm at room temperature, and the solid-state batteries retain over 87% of their capacity after 100 cycles at room temperature, achieving a specific capacity of 75-105 mAh / g at 1C rate. Furthermore, from... Figure 5 It can be seen that the solid-state battery in Example 1 does not catch fire or explode after being bent, cut, or punctured, and still maintains stable discharge, demonstrating excellent safety performance.
Claims
1. A method for preparing modified silica composite gel electrolyte, characterized in that: Includes the following steps: A. Dissolve plant polyphenols in deionized water to obtain a polyphenol solution; dissolve metal salts in deionized water to obtain a metal salt solution; dissolve a buffer in deionized water to obtain a buffer solution. B. Mix the polyphenol solution obtained in step A with the buffer solution, add silica, and sonicate evenly at room temperature. Then add the metal salt solution obtained in step A, stir and react at room temperature, and then centrifuge, wash and vacuum dry to obtain modified silica. C. Mix the modified silica, polymer monomer, lithium salt, initiator and organic solvent obtained in step B evenly to obtain a composite gel electrolyte precursor solution. D. The composite gel electrolyte precursor solution obtained in step C is subjected to in-situ polymerization to obtain modified silica composite gel electrolyte. In step A, the metal ion in the metal salt is Zn. 2+ The anion is selected from Cl. - NO3 - or SO4 2- At least one of them.
2. The preparation method of the modified silica composite gel electrolyte according to claim 1, characterized in that: In step A, at least one of the following conditions must be met: The plant polyphenols are selected from at least one of tannic acid, ellagic acid, catechin or gallic acid; The mass concentration of the polyphenol solution is 1~5 mg / mL; The metal salt is selected from zinc sulfate or zinc chloride; The mass concentration of the metal salt solution is 1~5 mg / mL; The buffer is selected from at least one of tris(hydroxymethyl)aminomethane, tris(hydroxymethyl)aminomethane hydrochloride, bis(2-hydroxyethylamino)tris(hydroxymethyl)methane, or bis(2-hydroxyethylamino)tris(hydroxymethyl)methane hydrochloride; The mass concentration of the buffer solution is 0.1~0.5 mg / mL.
3. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step B, the molar ratio of polyphenols in the polyphenol solution to metal salts in the metal salt solution is 1:20~40, the amount of buffer solution added is used to control the pH value of the system to 3~6, and the mass concentration of silica in the system is 1~10 mg / mL.
4. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step B, at least one of the following must be satisfied: The silicon dioxide is in the micro-nano scale; The time for ultrasonic dispersion to achieve uniformity is 30-60 minutes. The stirring reaction time is 6~36 hours; The stirring speed is 300~500 r / min; The vacuum drying temperature is 50~70℃; The vacuum drying time is 8-16 hours.
5. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step B, the stirring reaction takes 10-14 hours.
6. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step C, at least one of the following must be satisfied: The polymer monomer is a multifunctional acrylate monomer, selected from at least one of pentaerythritol tetraacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, or trimethylolpropane triacrylate. The initiator is an azo compound, selected from at least one of azobisisobutyronitrile, dimethyl azobisisobutyrate, or azobisisoheptanenitrile; The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide. The organic solvent is selected from at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, fluoroethylene carbonate, methyl butyrate, ethyl butyrate, or ethyl acetate.
7. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step C, the organic solvent is selected from a mixture of ethylene carbonate, methyl ethyl carbonate and diethyl carbonate in a volume ratio of 1:1:
1.
8. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step C, at least one of the following must be satisfied: The polymer monomer has a mass percentage of 3-8% in the composite gel electrolyte precursor solution; The initiator has a mass percentage of 0.1-0.5% in the composite gel electrolyte precursor solution; The concentration of the lithium salt in the composite gel electrolyte precursor solution is 0.8~1.2 mol / L; The modified silica has a mass percentage content of 0.01-5% in the composite gel electrolyte precursor solution.
9. The method for preparing the modified silica composite gel electrolyte according to claim 1, characterized in that: In step D, the temperature of the in-situ polymerization reaction is 50~80℃; the time of the in-situ polymerization reaction is 10~72h.
10. The modified silica composite gel electrolyte prepared by the method according to any one of claims 1 to 9.
11. The application of the modified silica composite gel electrolyte of claim 10 in in-situ gelled solid-state batteries.
12. An in-situ gelled solid-state battery, characterized in that: Its preparation method includes the following steps: The positive electrode, separator, and negative electrode are assembled into a battery, and then the composite gel electrolyte precursor solution obtained in step C of any one of claims 1 to 9 is injected. The battery is then sealed and subjected to in-situ polymerization to obtain the final product.
Citation Information
Patent Citations
Modified nano-SiO2 particles, their preparation methods, nanofiber membranes containing them, gel electrolytes, and lithium metal batteries.
CN108281705B
A modified nano-silica, its preparation method and application
CN111416146B
Modified silicon dioxide, solid electrolyte and lithium ion battery
CN115588773A
Nanometer composite polymer electrolyte for rechargeable lithium battery and its prepn process
CN1188466C
PH response type corrosion inhibition capsule based on metal polyphenol network structure and preparation and application of pH response type corrosion inhibition capsule
CN113774385A