Middle frame and manufacturing method thereof and electronic device

By using amorphous alloy and vapor deposition technology in the middle frame of electronic equipment to form a mirror appearance, combined with the annular depression area and injection molding process, the problems of weight and texture of the middle frame are solved, and high tensile strength and low density are achieved. Reduced manufacturing costs.

CN117714580BActive Publication Date: 2024-11-19HONOR DEVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310909499.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-11-19
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

It is difficult to take into account both the appearance texture and lightweight design of the existing electronic equipment. It has both the stainless steel vapour deposition technology that leads to increase weight, and the aluminum alloy and anode appearance technology that leads to poor texture.

Method used

Amorphous alloy is used as the frame material of the middle frame, and a mirror appearance is formed through vapor deposition technology. At the same time, annular depression area and a second frame with a density smaller than that of the amorphous alloy are set on the frame to reduce weight, combined with die casting and injection molding processes to improve the material Utilization and reduce manufacturing costs.

Benefits of technology

The high tensile strength and low density of the midframe are achieved, ensuring both appearance texture and lightweight, reducing manufacturing costs, and improving material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117714580B_ABST
    Figure CN117714580B_ABST
Patent Text Reader

Abstract

The embodiment of the present application provides a middle frame and a manufacturing method thereof and an electronic device, wherein the middle frame includes a frame and a middle plate, wherein the frame includes a first frame connected to the middle plate, wherein the molding material of the first frame includes an amorphous alloy, and the first frame is arranged around the peripheral edge of the middle plate. The side of the first frame away from the middle plate is a vapor deposition surface. The vapor deposition surface is a mirror surface and forms the appearance surface of the middle frame. The middle frame of the present application can take into account both the appearance texture and the lightweight design requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electronic technology, and in particular to a middle frame and a manufacturing method thereof and an electronic device. Background Art

[0002] With the development of electronic devices such as mobile phones and tablets, people not only have higher and higher requirements on the performance of electronic devices (such as structural strength), but also have higher and higher requirements on the appearance and weight of electronic devices.

[0003] The middle frame is the main supporting structure in electronic devices. In order to meet people's requirements for the performance, appearance and weight of electronic devices, the middle frame design with both lightweight advantages and appearance texture has become the main development direction of electronic devices. A middle frame is provided in the related art, which adopts a stainless steel plus physical vapor deposition (PVD) design to form a mirror appearance on the stainless steel middle frame to enhance the appearance texture of the middle frame, but the weight of the middle frame is relatively large. For this reason, another middle frame is provided in the related art, which adopts an aluminum alloy plus anode appearance design, and the anode appearance is used as the appearance surface of the middle frame. Compared with the previous middle frame, this middle frame is lighter, but the appearance texture is poorer.

[0004] Therefore, how to balance the appearance texture and lightness of the middle frame has become a technical problem to be solved. Summary of the invention

[0005] The present application provides a middle frame and a manufacturing method thereof, and an electronic device, which can take into account both the appearance texture and lightweight design requirements of the middle frame.

[0006] A first aspect of an embodiment of the present application provides a middle frame, which includes a frame and a middle plate, the frame including a first frame connected to the middle plate, the molding material of the first frame includes an amorphous alloy, and the first frame is arranged around the peripheral edge of the middle plate; a side of the first frame away from the middle plate is a vapor deposition surface, the vapor deposition surface is a mirror surface, and the vapor deposition surface forms the appearance surface of the middle frame.

[0007] By setting the vapor deposition surface on the first frame and the vapor deposition surface as a mirror, the texture of the appearance of the middle frame can be improved, and the appearance texture of the mirror surface at least equivalent to that of the middle frame with stainless steel and PVD treatment in the related art can be obtained, so as to meet the consumer's demand for the mirror appearance texture of the middle frame. In addition, by setting the amorphous alloy, while meeting the requirements of the tensile strength and other performances of the middle frame, when the material of the middle plate and the size of the middle frame are the same, the middle frame can also achieve a significant weight reduction compared with the middle frame with stainless steel and PVD treatment in the related art. Therefore, the middle frame of the present application can take into account both the appearance texture and lightweight design requirements of the middle frame.

[0008] In some optional embodiments, the first frame includes a frame body and a vapor deposition layer, the molding material of the frame body includes an amorphous alloy, the frame body is arranged around the peripheral edge of the middle plate and connected to the middle plate, and the side of the frame body away from the middle plate is a mirror surface; the vapor deposition layer is deposited on the mirror surface of the frame body to form a vapor deposition surface on the first frame.

[0009] Due to the mirror surface on the frame body, when the vapor deposition layer is deposited on the mirror surface of the frame body, a mirror vapor deposition surface can be formed on the first frame. In addition, since the molding material of the frame body includes an amorphous alloy, the frame body can be easily polished to form a mirror surface on the side away from the middle plate.

[0010] In some optional embodiments, the frame body includes a connecting portion and an enclosing portion connected to each other, wherein the connecting portion is arranged around the peripheral edge of the middle plate and connected to the middle plate;

[0011] The enclosing portion is arranged on a side of the connecting portion away from the middle plate, and forms a receiving space with the connecting portion and the middle plate.

[0012] In this way, the frame body is connected to the middle plate through the connecting portion to realize assembly with the middle plate, and the electronic components of the electronic equipment can also be easily accommodated in the accommodating space.

[0013] In some optional embodiments, the frame body is a die-casting of an amorphous alloy to form a first frame, thereby improving material utilization, shortening the processing time of the frame body, and reducing the manufacturing cost of the middle frame.

[0014] In some optional embodiments, one side of the first frame adjacent to the middle plate has at least one annular recessed area, and the frame also includes a second frame adapted to the shape of the recessed area, the second frame is accommodated in the recessed area and connected to the inner wall of the recessed area; the density of the molding material of the second frame is less than the density of the amorphous alloy.

[0015] By setting the recessed area and the second frame, the weight of the middle frame can be further reduced because the density of the molding material of the second frame is lower than the density of the amorphous alloy without affecting the overall structure, structural strength and reliability of the middle frame and the formation of the vapor deposition surface.

[0016] In some optional embodiments, the frame body of the first frame has an annular groove, which forms a recessed area, wherein along the thickness direction of the middle frame, the annular groove is distributed on at least one side of the middle plate and extends in a direction away from the middle plate, so as to increase the groove width of the annular groove and the volume ratio of the second frame in the frame, thereby enhancing the weight reduction effect of the middle frame.

[0017] In some optional embodiments, there are two annular grooves, which are distributed on opposite sides of the middle plate along the thickness direction of the middle frame and are symmetrically arranged on the frame body to further reduce the weight of the middle frame.

[0018] In some optional embodiments, the bottom of the annular groove is a plane, and the side wall of the annular groove transitions to the bottom of the groove in an arc shape, so as to facilitate die-casting of the frame body.

[0019] In some optional embodiments, the thickness of the frame body at the bottom of the groove and the side wall adjacent to the middle plate is greater than or equal to 0.3 mm and less than or equal to 5 mm, and the thickness of the frame body at the side wall away from the middle plate is greater than or equal to 0.15 mm, so as to facilitate the die-casting of the frame body while avoiding crystal solidification of the frame body during the die-casting process.

[0020] In some optional embodiments, the groove bottom and the side wall are connected by a rounded corner, and the radius of the rounded corner is greater than or equal to 0.2 mm to avoid the frame body being difficult to form during the die-casting process due to the rounded corner being too small.

[0021] In some optional embodiments, the second frame is located within the edge range of the first frame in the width direction of the middle plate, and the second frame and the middle plate together form a receiving space, so as to achieve further weight reduction of the middle frame while ensuring that the setting of the second frame does not affect the overall appearance of the frame and the middle frame.

[0022] In some optional embodiments, the second frame is an injection-molded part integrally connected to the first frame, and the molding material of the injection-molded part includes plastic particles with a density lower than that of the amorphous alloy, so that the second frame can be formed in the recessed area through the injection molding process while also reducing the average density and mass of the frame.

[0023] In some optional embodiments, the plastic particles include at least one of polycarbonate, polyethylene and polystyrene, so that the second frame can be formed by an injection molding process and the molding material of the second frame can be more diversified.

[0024] In some optional embodiments, the volume ratio of the second frame to the frame is 1 / 2 to 2 / 3, so as to enhance the weight reduction effect of the second frame on the center frame while meeting the structural strength and structural support requirements of the electronic device to the center frame.

[0025] In some optional embodiments, the amorphous alloy includes a zirconium-based amorphous alloy, so as to meet the requirements of the electronic device for the tensile strength and other properties of the middle frame, while also facilitating the grinding and polishing of the first frame and facilitating the formation of a vapor deposition surface.

[0026] In some optional embodiments, the tensile strength of the first frame is greater than 1400 MPa to meet the requirements of the electronic device for the tensile strength and other performance of the middle frame.

[0027] A second aspect of an embodiment of the present application provides a method for manufacturing a middle frame, the method comprising:

[0028] Forming an ingot into an amorphous alloy frame, the ingot being made of a master alloy;

[0029] The amorphous alloy frame is subjected to surface treatment to obtain a first frame, one side of the first frame forms a vapor deposition surface, and the vapor deposition surface is a mirror surface;

[0030] The first frame is arranged around the peripheral edge of the middle plate and connected with the middle plate to form a middle frame, and the vapor deposition surface is the appearance surface of the middle frame.

[0031] The middle frame obtained by the middle frame manufacturing method can obtain a first frame with ultra-high tensile strength and low density. On the basis of meeting the structural strength and lightweight requirements of the electronic device for the middle frame such as tensile strength, the mirror surface setting of the vapor deposition surface can also achieve the mirror appearance texture of the middle frame.

[0032] In some optional embodiments, the amorphous alloy frame includes a zirconium-based amorphous alloy frame, so that by utilizing the properties of the zirconium-based amorphous alloy, a vapor deposition surface is obtained on one side of the first frame, while also obtaining a first frame with ultra-high tensile strength and lower density.

[0033] In some optional embodiments, the raw materials of the master alloy include zirconium, copper, nickel, aluminum and at least one rare earth metal, so that ingots containing these raw materials can be made into zirconium-based amorphous alloy frames, and are beneficial to enhancing the tensile strength of the zirconium-based amorphous alloy frames.

[0034] In some optional embodiments, the ingot is made into an amorphous alloy frame, comprising:

[0035] The ingot is die-cast in a mold to obtain an amorphous alloy frame. The tensile strength of the amorphous alloy frame is greater than 1400MPa, so that after the outer contour of the frame body is obtained after die-casting, the master alloy can also form an amorphous alloy during the die-casting process, and the amorphous alloy frame has the performance of an amorphous alloy.

[0036] In some optional embodiments, the mold is a copper mold, and the ingot is die-cast in the mold, comprising:

[0037] melting the ingot at a first preset temperature;

[0038] After the ingot is melted, it is cooled to a second preset temperature and vacuum die-casted in a copper mold to obtain an amorphous alloy frame;

[0039] The first preset temperature is greater than the melting point of the master alloy, the second preset temperature is greater than or equal to the melting point of the master alloy, and the vacuum degree of vacuum die casting is 10 -2 ~10 -3 pa.

[0040] This ensures that the ingot is in a molten state so as to be vacuum die-casted in a copper mold to form a frame body, and also enables the ingot to form an amorphous alloy frame at a faster solidification speed during the die-casting process.

[0041] In some optional embodiments, before the ingot is made into an amorphous alloy frame, the manufacturing method further comprises:

[0042] Obtaining raw materials for master alloy;

[0043] Pre-melting at least a portion of the rare earth metal in the raw material and a portion of the zirconium element to obtain a pre-melted material;

[0044] The premelt and the remaining raw materials are smelted, and then poured to obtain an ingot.

[0045] In this way, after the ingot is die-cast, a zirconium-based amorphous alloy frame with a tensile strength greater than 1400 MPa can be obtained.

[0046] In some optional embodiments, the smelting process includes vacuum induction melting process, and the melting temperature of the vacuum induction melting process is 1900-2000°C and the melting time is 5-10 minutes to ensure that the pre-melted material and the remaining raw materials obtained can be fully melted at the above melting temperature and melting time for subsequent pouring.

[0047] In some optional embodiments, the amorphous alloy frame is subjected to surface treatment, including:

[0048] Processing the amorphous alloy frame to obtain a rough blank of the frame body;

[0049] A mirror surface is formed on a part of the surface of the rough blank of the frame body to obtain the frame body;

[0050] The mirror surface is subjected to physical vapor deposition treatment to form a vapor deposition surface on the mirror surface of the frame body, so that after the physical vapor deposition treatment, the first frame can have the appearance and texture of the mirror surface.

[0051] In some optional implementations, when the frame includes a second frame, the first frame is disposed before the peripheral edge of the middle plate, and the manufacturing method further includes:

[0052] The second frame is attached to the recessed area of ​​the first frame, the recessed area is located on the side of the first frame facing the middle plate, and the recessed area is annular, wherein the density of the second frame is less than that of the first frame.

[0053] In this way, by setting the second frame, the weight of the middle frame can be further reduced without affecting the overall structure, strength and formation of the vapor deposition surface of the middle frame.

[0054] In some optional implementations, attaching the second frame to the recessed area of ​​the first frame includes:

[0055] The second frame is injection molded in the recessed area to form an integrated structure with the first frame.

[0056] A third aspect of an embodiment of the present application provides a middle frame, which is obtained by any of the above manufacturing methods, so that the middle frame can meet the requirements of both lightweight and mirror-like appearance and texture.

[0057] The fourth aspect of the embodiment of the present application provides an electronic device, which includes a display screen, a back cover and a middle frame provided by any one of the above, and the middle frame is located between the display screen and the back cover. The setting of the middle frame in the electronic device can not only improve the appearance and texture of the electronic device, but also facilitate the lightweight design of the electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 A schematic diagram of the structure of an electronic device provided in an embodiment of the present application;

[0059] Figure 2 An exploded diagram of an electronic device provided in an embodiment of the present application;

[0060] Figure 3 A schematic diagram of the structure of a middle frame provided in an embodiment of the present application;

[0061] Figure 4 for Figure 3 A schematic diagram of the structure of the middle frame in another viewing angle;

[0062] Figure 5 for Figure 3 Enlarged view of part A in the middle;

[0063] Figure 6 A schematic diagram of the structure of another middle frame provided in an embodiment of the present application;

[0064] Figure 7 for Figure 6 Enlarged view of middle part B;

[0065] Figure 8 A schematic diagram of a process for manufacturing a middle frame provided in an embodiment of the present application;

[0066] Fig. 9 A schematic diagram of a process for producing an ingot provided in an embodiment of the present application;

[0067] Fig.10 A schematic diagram of the process of surface treatment of an amorphous alloy frame provided in an embodiment of the present application.

[0068] Description of reference numerals:

[0069] 100-electronic device; 1-middle frame; 11-frame; 111-first frame; 1111-frame body; 1112-connecting part; 1113-enclosing part; 1114-vapor deposition layer; 1115-vapor deposition surface; 1116-bottom of groove; 1117-side wall; 1118-rounded corner; 1119-antenna seam; 112-second frame; 12-middle plate; 121-partitioning part; 122-accommodating area; 13-connecting part; 14-plug interface;

[0070] 2-back cover; 3-display screen; 4-circuit board; 5-battery; 6-camera module. DETAILED DESCRIPTION

[0071] The terms used in the implementation section of this application are only used to explain the specific embodiments of this application and are not intended to limit this application.

[0072] To facilitate understanding, the relevant technical terms involved in the embodiments of the present application are first explained and illustrated.

[0073] Amorphous alloys, commonly known as liquid metals, are solidified by ultra-rapid cooling. When the alloy solidifies, the atoms do not have time to arrange themselves in order and crystallize. The resulting solid alloy has a long-range disordered structure. The molecules (or atoms, ions) that make up the substance do not have regular periodicity in space, and there are no grains or grain boundaries of crystalline alloys.

[0074] Amorphous alloys have extremely high strength. Taking zirconium (Zr)-based amorphous alloys as an example, the tensile strength of amorphous alloys is relatively high, generally greater than 1400MPa, which is about twice that of ordinary stainless steel. Among them, the density of 304 stainless steel (SUS304) is generally 7.93g / m 3 The density of 316 stainless steel (SUS316) is generally 7.98g / m 3 Depending on the composition, the density of amorphous alloys is between 6.1 and 6.9 g / m 3 In the range of 2000-2000mm, it is about 14% lighter than stainless steel (such as 304 stainless steel and 316 stainless steel). In addition, amorphous alloys such as zirconium-based amorphous alloys are also scratch-resistant and easy to polish. They can adapt to various surface treatments and achieve a mirror-like appearance that is equal to or even exceeds that of stainless steel.

[0075] The mirror-like appearance texture of a structural part can be understood as the surface of the structural part being able to present an appearance texture similar to that of mirror reflection. Taking stainless steel as an example, the mirror-like appearance texture of the structural part can be removed through surface treatments such as polishing to reflect the true color of the metal and present an appearance texture similar to that of mirror reflection. Generally, the surface roughness of stainless steel is less than or equal to 0.05μm, and the light reflectivity is greater than or equal to 90%, which can be called a "mirror". Surface roughness refers to the unevenness of the smaller spacing and tiny peaks and valleys on the surface of stainless steel, and the light reflectivity refers to the ratio of the reflected luminous flux to the incident luminous flux. Among them, the smaller the surface roughness of the stainless steel, the greater the light reflectivity, and the better the mirror effect.

[0076] 6 series aluminum alloy can be understood as aluminum-silicon-magnesium alloy, in which magnesium and silicon are the main alloying elements of 6 series aluminum alloy.

[0077] An embodiment of the present application provides an electronic device, which may include but is not limited to a mobile phone, a tablet computer (i.e., a pad), a virtual reality (VR) device, a laptop computer, a personal computer (PC), an ultra-mobile personal computer (UMPC), a handheld computer, a smart wearable device, and other electronic devices with a middle frame.

[0078] The structure of the electronic device will be further described below in conjunction with the accompanying drawings and embodiments.

[0079] See also Figure 1 and Figure 2 As shown, the electronic device 100 may include a middle frame 1 and a back cover 2 , wherein the back cover 2 is connected to one side of the middle frame 1 , and together with the middle frame 1 , provides a structural frame for the electronic device 100 .

[0080] refer to Figure 2 As shown, in some embodiments, the middle frame 1 includes a middle plate 12 and a frame 11 connected to each other, and the frame 11 is arranged around the peripheral edge of the middle plate 12 and together with the middle plate 12 constitutes the middle frame 1. The frame 11 includes a top frame, a left frame, a bottom frame and a right frame, and the top frame, the left frame, the bottom frame and the right frame can be connected end to end to form a square ring-shaped frame structure. The top frame 11, the left frame 11, the bottom frame 11 and the right frame 11 are all side frames in the middle frame 1.

[0081] refer to Figure 2 As shown, in some embodiments, when the electronic device 100 is a mobile phone, a tablet computer, etc., the electronic device 100 may also have a display function. In this case, the electronic device 100 further includes a display screen 3, which is mounted on a side of the middle frame 1 opposite to the back cover 2, so as to realize the display function of the electronic device 100. At least part of the structure of the frame 11 away from the middle plate 12 may be located on the side of the display screen 3 and the back cover 2, and exposed on the outer surface of the electronic device 100 to constitute the appearance surface of the middle frame 1.

[0082] Figure 1 and Figure 2 A middle frame 1 is shown in the figure to simplify the structure of the electronic device 100. In some embodiments, the number of the middle frames 1 can also be two, and the two middle frames 1 can be rotatably connected and equipped with a foldable display screen 3, so that the configuration of the electronic device 100 can be changed by the relative rotation of the two middle frames 1, and the electronic device 100 can be switched between the folded state and the flattened state, which can meet people's demand for a large display area of ​​the electronic device 100 and facilitate users to carry it.

[0083] The structure of the electronic device 100 of the present application is further described below by taking a middle frame 1 as an example.

[0084] The display screen 3 can be enclosed together with the middle frame 1 and the back cover 2 to form a receiving cavity (not shown in the figure). The receiving cavity can be used to receive electronic components such as the circuit board 4, the camera module 6, the battery 5, the microphone, the speaker, and the receiver of the electronic device 100. The arrangement positions of the electronic components such as the circuit board 4, the camera module 6, the battery 5, the microphone, the speaker, and the receiver in the receiving cavity can refer to the relevant arrangements in the existing electronic device 100, and will not be repeated here.

[0085] The circuit board 4 can be understood as the mainboard of the electronic device 100 (such as a mobile phone). The circuit board 4 usually carries electronic devices such as a processor module, various controller modules, a storage module, a communication module, a radio frequency module, and a power management module.

[0086] The display screen 3 can be electrically connected to the circuit board 4 so that the display screen 3 can realize the display or operation function. The camera module 6 can be arranged on the circuit board 4 and electrically connected to the circuit board 4, so that when the user inputs a shooting instruction, the camera module 6 can be controlled by the circuit board 4 to shoot the target object, thereby realizing the shooting function of the electronic device 100.

[0087] The structure of the electronic device 100 of the embodiment of the present application is further described below by taking a mobile phone as an example.

[0088] The middle frame 1 is the main supporting structure of the sandwich structure in the electronic device 100. It not only needs a certain structural strength, but also part of the frame 11 is exposed on the outer surface of the electronic device 100, so that the middle frame 1, as an appearance part, also needs to have a sufficient appearance. Taking a mobile phone as an example, the middle frame 1, the display screen 3 and the back cover 2 form a sandwich structure of the electronic device 100. The middle frame 1 is the middle layer of the sandwich structure in the electronic device 100, mainly supporting the display screen 3 and the back cover 2.

[0089] In recent years, consumers have increasingly higher requirements not only for the performance of electronic devices such as mobile phones, but also for their weight and appearance. Therefore, the design of the middle frame that combines the advantages of lightweight and appearance texture has become the main development direction of the structural parts of electronic devices in order to meet people's requirements for the weight and appearance of electronic devices.

[0090] At present, the first related technology provides a first middle frame, which is made of stainless steel. After the appearance surface of the first middle frame is polished to a mirror surface, a physical vapor deposition (PVD) process is performed on the appearance surface of the first middle frame, so that the appearance surface of the first middle frame reaches the appearance texture of the mirror surface and has a high glossiness, which can improve the appearance texture of the first middle frame. In the present application, the surface roughness corresponding to the mirror surface of the first middle frame is not further limited. In this way, the first middle frame not only has the characteristics of high wear resistance and high corrosion resistance, but also the anti-drop impact ability of the first middle frame is also advantageously guaranteed.

[0091] However, since the density of stainless steel is usually greater than or equal to 7.8g / m 3 , which is about 3 times that of metal aluminum, resulting in a significant increase in the weight of the first middle frame compared to the aluminum alloy middle frame of the same size, reducing consumers' experience of using electronic devices.

[0092] To this end, the second related technology provides a second middle frame, which is made of 6 series aluminum alloy by a computer numerical control (CNC) machine tool, and an anodized surface treatment is performed on the exterior surface of the second middle frame to enhance the texture of the exterior surface of the second middle frame.

[0093] The density of the second middle frame is about 2.7g / cm 3 Compared with the first middle frame, the second middle frame has the advantage of being lightweight, but the CNC processing time is longer, the material utilization rate is lower, and the manufacturing cost is higher. In addition, the anode appearance is a non-mirror appearance. Due to the high difficulty of grinding and polishing aluminum alloy, it is difficult to achieve a mirror appearance on the second middle frame, making the texture of the second middle frame on the appearance surface inferior to that of the first middle frame on the appearance surface, and there is a certain gap between the appearance texture of the second middle frame and the first middle frame on the appearance surface.

[0094] Therefore, how to achieve both lightweight of the middle frame and a mirror-like appearance has become a technical problem to be solved.

[0095] In view of this, an embodiment of the present application provides a middle frame 1, which includes a frame 11 and a middle plate 12 that are interconnected. The main raw material of the frame 11 includes an amorphous alloy, so that through the setting of the amorphous alloy, not only can the middle frame 1 have a mirror appearance and texture, but also can achieve the effect of weight reduction, thereby reducing the manufacturing cost of the middle frame 1, and has great application prospects in electronic devices 100.

[0096] The structure of the middle frame 1 is further described below in conjunction with the accompanying drawings and embodiments.

[0097] See also Figure 3 As shown, the middle frame 1 includes a frame 11 and a middle plate 12, the frame 11 includes a first frame 111 connected to the middle plate 12, the molding material of the first frame 111 includes an amorphous alloy, and the first frame 111 is arranged around the peripheral edge of the middle plate 12. The side of the first frame 111 away from the middle plate 12 is a vapor deposition surface 1115, the vapor deposition surface 1115 is a mirror surface, and the vapor deposition surface 1115 forms the appearance surface of the middle frame 1, so that the texture of the appearance surface of the middle frame 1 can be improved by setting the vapor deposition surface 1115 on the first frame 111, and the appearance surface of the middle frame 1 can at least achieve the appearance texture of the mirror surface equivalent to the appearance surface of the first middle frame, so as to meet the consumer's demand for the appearance texture of the mirror surface of the middle frame 1.

[0098] It should be noted that the side of the first frame 111 away from the middle plate 12 may include the end face of the first frame 111 away from the middle plate 12 in the X direction. At this time, the vapor deposition surface 1115 is located on the end face of the first frame 111 away from the middle plate 12 in the X direction and forms the appearance surface of the middle frame 1.

[0099] Alternatively, in some embodiments, the side of the first frame 111 away from the middle plate 12 can also be understood as the outer peripheral surface of the first frame 111. The outer peripheral surface of the first frame 111 includes not only the end surface of the first frame 111 away from the middle plate 12 in the X direction, but also the outer surface of the first frame 111 away from the middle plate 12 in the Z direction. At this time, the vapor deposition surface 1115 is located on the outer peripheral surface of the first frame 111 and forms the appearance surface of the middle frame 1.

[0100] The structure of the middle frame 1 is further described below by taking the example that the vapor deposition surface 1115 is located on the outer peripheral surface of the first frame 111 .

[0101] Amorphous alloys not only have high strength, but also have lower density than stainless steel. Therefore, when the material of the middle plate 12 and the size of the middle frame 1 are the same, compared with the first middle frame described above, the first frame 111 can have a lower density by setting the amorphous alloy in the first frame 111, thereby reducing the weight of the middle frame 1 and meeting the requirements of the electronic device 100 for the tensile strength and other performance of the middle frame 1, while also being able to obtain a mirror-like appearance texture at least equivalent to that of the first middle frame. Therefore, the middle frame of the present application can take into account both the appearance texture and lightweight design requirements of the middle frame.

[0102] Moreover, compared to the second type of middle frame mentioned above, the appearance surface of the middle frame 1 of the present application not only has a mirror appearance texture, but also utilizes the characteristics of amorphous alloys that are scratch-resistant and easy to grind and polish. While making the first frame 111 easy to grind and polish to form a vapor deposition surface 1115, it can also reduce the processing difficulty of the first frame 111 and reduce the manufacturing cost of the middle frame 1.

[0103] The tensile strength of the first frame 111 is greater than 1400 MPa, so that the first frame 111 has a relatively high tensile strength to meet the requirements of the electronic device 100 for the tensile strength and other performances of the middle frame 1 .

[0104] The amorphous alloy may include a zirconium-based amorphous alloy or other amorphous alloys that are easy to grind and polish, have a tensile strength greater than 1400 MPa, and are scratch-resistant, so as to meet the requirements of the electronic device 100 for the tensile strength and other properties of the middle frame 1, while also facilitating the grinding and polishing of the first frame 111, and facilitating the formation of the vapor deposition surface 1115, ensuring that the appearance of the middle frame 1 can at least achieve the same mirror appearance texture as the first middle frame. In the present application, the type of amorphous alloy is not further limited.

[0105] The structure of the middle frame 1 of the present application is further described below by taking zirconium-based amorphous alloy as an example.

[0106] See also Figure 3As shown, in some embodiments, the middle plate 12 may be a metal middle plate, and the molding material of the metal middle plate may be a lightweight metal such as an aluminum alloy or a magnesium alloy, so as to further reduce weight and increase the lightweight advantage of the middle frame 1.

[0107] Alternatively, in other embodiments, the molding material of the middle plate 12 may also be plastic or may include both plastic and the above-mentioned light metal, etc. In the present application, the material and molding method of the middle plate 12 are not further limited.

[0108] See also Figure 4 As shown, as described above, the middle frame 1 can enclose a receiving cavity together with the display screen 3 and the back cover 2. In order to facilitate the arrangement of electronic devices such as the circuit board 4 and the battery 5 in the electronic device 100 in the receiving cavity, at least two strip-shaped partitions 121 can be provided on the plate surface of the middle plate 12 on the side facing the back cover 2. The partitions 121 can be provided on the middle plate 12 along at least one of the length direction and the width direction of the middle frame 1, so that the receiving cavity on the side of the middle plate 12 facing the back cover 2 is divided into a plurality of receiving areas 122 by at least one partition 121, so that the circuit board 4, the battery 5 and other electronic devices can be arranged in their respective corresponding receiving areas 122. In the present application, the arrangement position of the partition 121 and the corresponding receiving area 122 of the electronic device in the receiving cavity are not further limited.

[0109] It should be noted that, in some other embodiments, the accommodating cavity may be divided by partially providing a recessed structure on the middle plate 12 .

[0110] See also Figure 4 As shown, in order to facilitate the electrical connection between the electronic device 100 and external devices such as a socket, a plug interface 14 is also provided at the bottom of the middle frame 1, so that when a data interface such as a Universal Serial Bus (USB) is provided on the circuit board 4, it can be inserted into the plug interface 14 and electrically connected to an external device such as a socket.

[0111] In some embodiments, an antenna slot 1119 may be further provided on the peripheral side of the first frame 111 to prevent the middle frame 1 from shielding the signal of the electronic device 100 , so as to realize the communication function of the electronic device 100 such as a mobile phone.

[0112] The structural shape of the first frame 111 is a square ring structure that matches the structural shape of the frame 11. Specifically, the first frame 111 may be formed by connecting a plurality of side frames end to end. Please refer to the above structural description of the frame 11 and no further limitation is made here.

[0113] Figure 5 Indicated Figure 3 The enlarged view of part A is provided to facilitate observation of the structure of the frame 11 .

[0114] See also Figure 5 As shown, the first frame 111 may include a frame body 1111 and a vapor deposition layer 1114 . The molding material of the frame body 1111 may be the same as the molding material of the first frame 111 , which will not be further described herein.

[0115] The frame body 1111 is arranged around the peripheral edge of the middle plate 12 and connected to the middle plate 12, and the side of the frame body 1111 away from the middle plate 12 is a mirror surface. The vapor deposition layer 1114 is deposited on the mirror surface of the frame body 1111 to form a vapor deposition surface 1115 on the first frame 111. Due to the setting of the mirror surface on the frame body 1111, when the vapor deposition layer 1114 is deposited on the mirror surface of the frame body 1111, the vapor deposition surface 1115 can be formed on the first frame 111, so that the appearance surface of the middle frame 1 can at least achieve the appearance texture of the mirror surface equivalent to the first type of middle frame.

[0116] Since the molding material of the frame body 1111 includes an amorphous alloy, the frame body 1111 can be easily polished to form a mirror surface on the side away from the middle plate 12, so that after the vapor deposition layer 1114 is deposited, a vapor deposition surface 1115 is formed, which can reduce the processing difficulty of the first frame 111.

[0117] It should be noted that the mirror surface of the frame body 1111 can be understood as a surface with a mirror-like reflection effect after grinding and polishing on the frame body 1111. In the present application, no further limitation is imposed on the surface roughness of the frame body 1111 on the mirror surface, as long as the mirror effect of the frame body 1111 can be at least equivalent to the mirror effect of the first middle frame before PVD treatment.

[0118] The vapor deposition layer 1114 can be obtained by performing PVD treatment on the mirror surface of the frame body 1111. After the PVD treatment, a vapor deposition surface 1115 can be formed on the mirror surface, and the frame body 1111 has a higher gloss on the vapor deposition surface 1115 to enhance the appearance texture of the middle frame 1. The PVD treatment process on the mirror surface can refer to the relevant process in the first middle frame, and will not be further described in this application. This application does not further limit the thickness of the vapor deposition layer 1114, as long as a relatively uniform vapor deposition surface 1115 can be formed on the mirror surface.

[0119] See also Figure 5As shown, the frame body 1111 includes a connecting portion 1112 and an enclosure portion 1113 that are interconnected. The connecting portion 1112 is arranged around the peripheral edge of the middle plate 12 and is connected to the middle plate 12. The enclosure portion 1113 is arranged on the side of the connecting portion 1112 away from the middle plate 12, and forms a receiving space with the connecting portion 1112 and the middle plate 12. In this way, the frame body 1111 is connected to the middle plate 12 through the connecting portion 1112 to achieve assembly with the middle plate 12, and electronic devices such as the circuit board 4, the camera module 6, the battery 5, the microphone, the speaker or the earpiece can be received in the receiving space. The connection 13 between the connecting portion 1112 and the middle plate 12 can be seen in FIG. Figure 4 and Figure 5 shown.

[0120] It should be noted that when the display screen 3 and the back cover 2 are disposed on a side of the receiving space away from the middle plate 12 and connected to the enclosure 1113 , they can respectively form a receiving cavity with the middle plate 12 .

[0121] See also Figure 5 Combined with Figure 4 As shown, the connecting portion 1112 may be a square ring structure disposed around the edge of the middle plate 12, and the enclosing portion 1113 may also be a square ring structure disposed around the connecting portion 1112. The cross-sectional shape of the frame body 1111 on one side of the middle plate 12 may be a "T" shape, so as to achieve the connection between the frame body 1111 and the middle plate 12.

[0122] The connection part 1112 can be connected to each other by welding, riveting, nano injection molding or adhesive structure, so as to complete the assembly of the first frame 111 and the middle plate 12 to form a complete middle frame 1. Alternatively, in other embodiments, the connection part 1112 can be assembled with the middle plate 12 by welding and adhesive structure to form a complete middle frame 1.

[0123] It should be noted that the glue-drawing structure can be understood as a connection method of glue point or other glue connection. The connection method of the first frame 111 and the middle plate 12 is not further limited here.

[0124] The surface of the enclosing portion 1113 on the side away from the connecting portion 1112 can be polished to form a mirror surface of the frame body 1111 so that the vapor deposition layer 1114 can be deposited on the mirror surface of the frame body 1111 and form the appearance surface of the middle frame 1.

[0125] The frame body 1111 is a die-casting of an amorphous alloy to form the first frame 111. Compared with the second middle frame, since the frame body 1111 is a die-casting formed by a die-casting process, it is possible to reduce the cutting waste generated during the manufacturing process of the frame body 1111, improve the material utilization rate, shorten the processing time of the frame body 1111, and reduce the manufacturing cost of the middle frame 1. Among them, the interest rate of the material of the second middle frame in the manufacturing process is generally about 40%, while the interest rate of the material of the middle frame 1 of the present application is at least greater than or equal to 70%.

[0126] Since the amorphous alloy is used as the molding material of the first frame 111 , the high strength characteristic thereof can meet the structural strength and reliability requirements of the middle frame 1 of electronic devices 100 such as mobile phones with a large redundancy.

[0127] Therefore, in order to further reduce the weight of the middle frame 1, see Figure 6 As shown, in other embodiments, one side of the first frame 111 adjacent to the middle plate 12 has at least one annular recessed area (not shown in the figure), and the frame 11 also includes a second frame 112 that matches the shape of the recessed area, and the second frame 112 is accommodated in the recessed area and connected to the inner wall of the recessed area. The density of the molding material of the second frame 112 is less than the density of the amorphous alloy. In this way, the higher strength characteristics of the amorphous alloy can be effectively utilized, and the recessed area can be compensated by setting the second frame 112 in the recessed area. Without affecting the overall structure, structural strength and reliability of the middle frame 1 and the formation of the vapor deposition surface 1115, the weight reduction of the frame 11 and the middle frame 1 can be further achieved.

[0128] It should be noted that the shape of the second frame 112 is adapted to the recessed area, which can be understood as the second frame 112 being the same or similar in shape to the recessed area, so that the second frame 112 can be accommodated in the recessed area while avoiding the setting of the second frame 112 affecting the structure of the frame 11, thereby ensuring the consistency of the overall structure of the middle frame 1.

[0129] The recessed area can be located on the side of the frame body 1111 facing the middle plate 12, and is arranged on the side of the enclosure portion 1113 that is connected to the connecting portion 1112, so as to achieve weight reduction of the frame 11 and the middle frame 1 without affecting the shape of the appearance surface of the middle frame 1.

[0130] See also Figure 7As shown, the second frame 112 is located within the edge range of the first frame 111 in the width direction of the middle plate 12, and the width direction of the middle plate 12 can refer to the above-mentioned X direction. The second frame 112 and the middle plate 12 together enclose a receiving space, so that by setting the second frame 112, the frame 11 and the middle frame 1 are further reduced in weight. Since the second frame 112 is located within the projection range of the first frame 111 on the middle plate 12, it can also be ensured that the setting of the second frame 112 will not affect the overall appearance of the frame 11 and the middle frame 1.

[0131] In some embodiments, Figure 7 As shown, in some embodiments, the edge of the second frame 112 facing the middle plate 12 can be flush with the first frame 111 to ensure that the second frame 112 can be located within the edge range of the first frame 111 in the width direction of the middle plate 12.

[0132] The second frame 112 can be an injection-molded part integrally connected to the first frame 111. The molding material of the injection-molded part includes plastic particles with a density lower than that of the amorphous alloy, so that the second frame 112 can be formed in the recessed area through the injection molding process. While enhancing the connection strength between the second frame 112 and the first frame 111 and the tensile strength of the frame 11, the average density and mass of the frame 11 can be reduced. When the material of the middle plate 12 and the size of the middle frame 1 remain unchanged, at least compared with the first middle frame, the frame 11 and the middle frame 1 can be significantly reduced in weight.

[0133] The plastic particles may include at least one of polycarbonate (PC), polyethylene (PE) and polystyrene (PS), so that after the injection molding process, the second frame 112 having a density less than that of the first frame 111 can be formed, and the molding material of the second frame can be more diversified. Alternatively, in some embodiments, the plastic particles may also be other plastic particles having a density less than that of amorphous alloys. In the present application, the type of plastic particles is not further limited.

[0134] The volume ratio of the second frame 112 in the frame 11 is 1 / 2 to 2 / 3, that is, 1 / 2 to 2 / 3 of the volume of the frame 11 is filled with plastic particles. For example, the volume ratio of the second frame 112 in the frame 11 can be 1 / 2 or 2 / 3. By limiting the volume ratio of the second frame 112 in the frame 11, it is possible to avoid the volume ratio of the second frame 112 in the frame 11 being too small, which limits the weight reduction effect of the frame 11 and the middle frame 1, and it is also possible to avoid the volume ratio of the second frame 112 in the frame 11 being too large, which affects the structural strength of the middle frame 1.

[0135] Therefore, the present application limits the upper and lower limits of the volume ratio of the second frame 112 to the frame 11, so that on the basis of meeting the requirements of the electronic device 100 for the structural strength and structural support of the middle frame 1, the average density and mass of the frame 11 can be significantly reduced, thereby enhancing the weight reduction effect of the second frame 112 on the frame 11 and the middle frame 1.

[0136] It should be noted that when the frame 11 includes the first frame 111, the average density of the frame 11 may be the density of the first frame 111. Taking zirconium-based amorphous alloy as an example, the average density of the frame 11 may be 6.1 to 6.9 g / m 3 within the range.

[0137] Taking PC as an example, when the volume ratio of the second frame 112 in the frame 11 is 1 / 2 to 2 / 3, the average density of the frame 11 can be less than the density of the first frame 111. When the frame 11 includes the first frame 111 and the second frame 112, and the middle plate 12 uses the same metal middle plate as the first middle frame, the average density of the middle frame 1 of the present application can be reduced to 2.5 to 3.1 g / m 3 , so that the weight difference between the middle frame 1 and the second middle frame mentioned above is small, and compared with the first middle frame, it can achieve significant weight reduction, so as to better meet the lightweight design requirements of the middle frame 1.

[0138] See also Figure 7 As shown, the recessed area may be an annular groove on the frame body 1111, and the annular groove forms a recessed area so as to accommodate the second frame 112 in the first frame 111, thereby further reducing the weight of the middle frame 1. At this time, the frame body 1111 and the portion of the first frame 111 on either side of the middle plate 12 may form an "E"-shaped structure. Alternatively, in other embodiments, the recessed area may also be a concave-convex structure on the inner wall of the first frame 111, which can also further reduce the weight of the middle frame 1. In the present application, the structure of the recessed area is not further limited.

[0139] Figure 7 The structure of the annular groove on the first frame 111 is illustrated in the figure. Compared with the concave-convex structure of the recessed area, by opening the annular groove, while ensuring that the tensile strength and other properties of the middle frame 1 can meet the requirements of the electronic device 100, more space in the first frame 111 can be released to further enhance the weight reduction effect of the second frame 112 on the middle frame 1.

[0140] The structure of the middle frame 1 is further described below by taking the annular groove as an example.

[0141] See also Figure 7As shown, along the thickness direction of the middle frame 1, the annular groove is distributed on at least one side of the middle plate 12 and extends in the direction away from the middle plate 12 (Z direction), so as to increase the groove width of the annular groove and the volume ratio of the second frame 112 in the frame 11, thereby enhancing the weight reduction effect of the frame 11 and the middle frame 1. Figure 7 The Z direction in .

[0142] like Figure 7 As shown, in some embodiments, there may be two annular grooves, which are distributed on opposite sides of the middle plate 12 along the thickness direction of the middle frame 1 and are symmetrically arranged on the frame body 1111. At this time, there are also two second frames 112, which correspond to one annular groove respectively and are accommodated in the corresponding annular groove and connected to the inner wall of the annular groove to form the frame 11, so that the two second frames 112 are also symmetrically arranged on the first frame 111 along the thickness direction (Z direction) of the middle frame 1.

[0143] It should be noted that, compared with the first middle frame described above, the middle frame 1 of the present application can further reduce weight by providing two annular grooves and two second frames 112, provided that the material of the middle plate 12 and the size of the middle frame 1 are the same. For example, the middle frame 1 of the present application can reduce weight by at least 51%. In some quality tests on the middle frame 1, compared with the first middle frame described above, the middle frame 1 of the present application can reduce weight by about (approximately or approximately) 53%.

[0144] Alternatively, the first frame 111 may also have an annular groove, and along the thickness direction of the middle frame 1, the annular groove may be distributed on any side of the middle plate 12, which can also achieve further weight reduction of the frame 11 and the middle frame 1 compared to the first type of middle frame mentioned above.

[0145] See also Figure 7 As shown, the bottom 1116 of the annular groove can be a plane, and the side wall 1117 of the annular groove transitions to the bottom 1116 in an arc shape, so that the frame body 1111 can be die-casted to form the first frame 111 after grinding, polishing and PVD treatment.

[0146] Specifically, the groove bottom 1116 and the side wall 1117 may be connected by a fillet 1118 , and the radius of the fillet 1118 may be greater than or equal to 0.2 mm to prevent the fillet 1118 from being too small, making it difficult to form the frame body 1111 during the die-casting process.

[0147] The annular groove includes two side walls 1117. For the convenience of description, the two side walls 1117 are respectively defined as the first side wall and the second side wall. The fillet 1118 between the first side wall and the groove bottom 1116 can be called the inner fillet, and the fillet 1118 between the second side wall and the groove bottom 1116 can be called the outer fillet. The inner fillet and the outer fillet can be the same or different. In the present application, no further limitation is made to this, as long as the radii of the inner fillet and the outer fillet are both greater than or equal to 0.2 mm.

[0148] The thickness of the frame body 1111 at the groove bottom 1116 and the side wall 1117 adjacent to the middle plate 12 is greater than or equal to 0.3 mm and less than or equal to 5 mm. The thickness of the frame body 1111 at the groove bottom 1116 can be represented by D1. Among them, the thickness of the frame body 1111 at the side wall 1117 adjacent to the middle plate 12 can be understood as the thickness of the frame body 1111 at the first side wall, which can be represented by D2. Both D1 and D2 can be understood as the thickness of the first frame 111 at a larger plane. For example, the thickness of the first frame 111 at a larger plane can be 0.3 mm, 0.5 mm, 1 mm, 1.5 mm, 2 mm, 3 mm, 3.5 mm, 4 mm or 5 mm, etc.

[0149] By limiting the thickness of the first frame 111 at a larger plane, it is possible to avoid the first frame 111 being too thin at a larger plane, which would make the frame body 1111 difficult to die-cast. It is also possible to avoid the first frame 111 being too thick at a larger plane, which would result in a lower central cooling rate of the frame body 1111 during the die-casting process and easy crystal solidification, thereby making it difficult for the performance of the amorphous alloy, the molding material of the frame body 1111, to meet the standards.

[0150] The thickness of the first frame 111 at the side wall 1117 away from the middle plate 12 is greater than or equal to 0.15 mm. The thickness of the first frame 111 at the side wall 1117 away from the middle plate 12 can be understood as the thickness of the first frame 111 at the second side wall, which can be represented by D3. D3 can be understood as the thickness of the first frame 111 at a smaller plane. For example, the thickness of the first frame 111 at a smaller plane can be 0.15 mm, 0.2 mm, 0.3 mm, or greater than 0.3 mm.

[0151] In the present application, the upper limit of the thickness of the first frame 111 at the smaller plane is not further limited. By limiting the lower limit of the thickness of the first frame 111 at the smaller plane, the die-casting of the frame body 1111 can be ensured while the annular groove extends in a direction away from the middle plate 12, increasing the groove width of the annular groove and the volume ratio of the second frame 112 in the frame 11.

[0152] On the basis of the above, the present application further provides a method for manufacturing a middle frame 1, so as to obtain the middle frame 1 of the present application according to the manufacturing method.

[0153] The manufacturing method of the middle frame 1 is further described below in conjunction with the accompanying drawings and embodiments.

[0154] See also Figure 8 As shown, the production method includes:

[0155] Step S100: forming an amorphous alloy frame from an ingot, wherein the ingot is made of a master alloy;

[0156] Step S200: performing surface treatment on the amorphous alloy frame to obtain a first frame, wherein one side of the first frame forms a vapor deposition surface, and the vapor deposition surface is a mirror surface;

[0157] Step S300: a first frame is disposed around the peripheral edge of the middle plate and connected with the middle plate to form a middle frame, and the vapor deposition surface is the appearance surface of the middle frame.

[0158] It should be noted that during the process of casting the ingot into an amorphous alloy frame, the master alloy will form an amorphous alloy and make the amorphous alloy frame have the properties of an amorphous alloy. This not only facilitates the surface treatment of the amorphous alloy frame, but also obtains a vapor deposition surface 1115 on one side of the first frame 111.

[0159] Moreover, after step S200, a first frame 111 with ultra-high tensile strength and low density can be obtained, so that the lightweight and mirror-like appearance of the middle frame 1 can be achieved while satisfying the requirements of the electronic device 100 for the structural strength of the middle frame 1 such as the tensile strength.

[0160] The amorphous alloy frame may include a zirconium-based amorphous alloy frame, that is, the amorphous alloy frame may be made of a zirconium-based amorphous alloy, so as to utilize the performance of the zirconium-based amorphous alloy, and at the same time as obtaining a vapor deposition surface 1115 on one side of the first frame 111, a first frame 111 with ultra-high tensile strength and low density can be obtained, so as to achieve lightweight and mirror-like appearance of the middle frame 1. The performance of the zirconium-based amorphous alloy and the amorphous alloy can be referred to the relevant description above, and will not be repeated here.

[0161] Alternatively, in other embodiments, the amorphous alloy frame may also be made of other amorphous alloys that are easy to grind and polish, have a tensile strength greater than 1400 MPa, and are scratch-resistant. In this application, the molding material of the amorphous alloy frame is not further limited.

[0162] The following is a further description of the manufacturing method of the present application by taking a zirconium-based amorphous alloy frame as an example.

[0163] The raw materials of the master alloy may include zirconium (Zr), copper (Cu), nickel (Ni), aluminum (Al) and at least one rare earth metal. The molar fraction of Zr in the master alloy is greater than the molar fraction of Cu, Ni, Al or rare earth metal in the master alloy, so that Zr is the main raw material of the master alloy, and the master alloy containing these raw materials is beneficial to enhancing the tensile strength of the zirconium-based amorphous alloy frame after being made into a zirconium-based amorphous alloy frame.

[0164] The rare earth metals may include other rare earth metals such as hafnium (Hf) and niobium (Nb). The amorphous alloy made from the master alloy of these raw materials is Zr a Cu b Ni c Al d Q e , Q includes a general formula of one or at least two rare earth metals, and a, b, c, d and e are the mole fractions of the corresponding raw materials. When Q contains two or more rare earth metals, the sum of the mole fractions of the rare earth metals in the raw materials in the master alloy is e. The sum of the mole fractions of the raw materials in the master alloy is 100.

[0165] In some embodiments, in addition to the above raw materials, the raw materials of the master alloy may also include iron (Fe) or titanium (Ti) to make the composition of the zirconium-based amorphous alloy frame more diverse. When the raw materials of the master alloy may also include iron, the amorphous alloy made from the master alloy containing these raw materials is Zr a Cu b Ni c Al d Fe f Q e , f is the molar fraction of Fe. When the raw materials of the master alloy can also include titanium, the amorphous alloy made from the master alloy containing these raw materials is Zr a Cu b Al d Ti g Ni c Q e , g is the molar fraction of Ti. In the present application, the type of raw materials of the master alloy is not further limited, as long as it can form a zirconium-based amorphous alloy frame.

[0166] It should be noted that in the prior art, the zirconium-based amorphous alloy with a tensile strength greater than 1400MPa has many components and is difficult to further restrict. One of the protection points of this application is to use the first frame 111 made of a zirconium-based amorphous alloy, rather than protecting the components of the zirconium-based amorphous alloy. Therefore, in this application, the types and molar fractions of the raw materials in the master alloy are not limited, as long as the zirconium-based amorphous alloy with a tensile strength greater than 1400MPa can be obtained after die-casting.

[0167] In step S100, the ingot is made into an amorphous alloy frame, which may specifically include:

[0168] The ingot is die-cast in a mold to obtain an amorphous alloy frame. The tensile strength of the amorphous alloy frame is greater than 1400MPa. During the die-casting of the ingot in the mold, after obtaining the outer contour of the frame body 1111, the master alloy can also form an amorphous alloy during the die-casting process, and make the amorphous alloy frame have the properties of an amorphous alloy, so as to achieve the lightweight of the middle frame 1 and the mirror-like appearance texture.

[0169] It should be noted that the tensile strength of the amorphous alloy frame mainly depends on the raw materials contained in the master alloy and the solidification rate of the ingot during the die-casting process. The solidification rate can also be called the cooling rate. The faster the solidification rate, the easier it is for the master alloy to form an amorphous state during the die-casting process of the ingot, and thus it is easier to obtain an amorphous alloy frame after the die-casting is completed.

[0170] Therefore, after the master alloy contains the above raw materials, an amorphous alloy frame with tensile strength meeting the requirements can be obtained by die-casting the ingot in a mold.

[0171] In addition, the heat conduction effect of the mold will affect the solidification speed of the ingot during the die casting process. Therefore, in order to ensure that the ingot has a faster solidification speed during the die casting process, the mold can be a copper mold or other metal molds with good heat conduction effect, so that the ingot has a faster solidification speed during the die casting process, so that the ingot made of the master alloy can form an amorphous alloy frame at a faster solidification speed during the die casting process. In this application, the type of mold is not further limited.

[0172] Taking the copper mold as an example, the die-casting process of the ingot in the mold is further explained below.

[0173] The ingot is die-cast in a mold, which includes:

[0174] melting the ingot at a first preset temperature;

[0175] After the ingot is melted, it is cooled to a second preset temperature and vacuum die-casted in a copper mold to obtain an amorphous alloy frame;

[0176] The first preset temperature is greater than the melting point of the master alloy, the second preset temperature is greater than or equal to the melting point of the master alloy, and the vacuum degree of vacuum die casting is 10 -2 ~10 -3 pa.

[0177] In this way, by setting the first preset temperature, it can be ensured that the ingot will be fully melted to form a molten state at the first preset temperature. After the ingot is melted, it is cooled to the second preset temperature for treatment. While ensuring that the ingot is still in a molten state so that the ingot can be vacuum die-cast in a copper mold, it can also reduce heat waste.

[0178] It should be noted that, taking the first frame 111 as an example of a zirconium-based amorphous alloy frame, the first preset temperature can be 1100-1300°C, and the second preset temperature can be 750-950°C. When the first frame 111 is an amorphous alloy frame that meets other requirements, the first preset temperature and the second preset temperature will also change accordingly. In this application, the first preset temperature and the second preset temperature are not further limited. The smelting of the ingot can be carried out in a vacuum melting furnace or other smelting device.

[0179] The molten ingot can be vacuum die-casted in a vacuum die-casting device with a copper mold. -2 ~10 -3 When vacuum die casting is carried out under pa, due to the presence of the copper mold, the ingot can have a faster solidification speed during the die casting process, so that an amorphous alloy frame with a tensile strength greater than 1400MPa can be obtained after the vacuum die casting is completed.

[0180] The amorphous alloy frame has the same or similar outer contour as the frame body 1111 and the first frame 111. The amorphous alloy frame can be understood as a rough blank of the frame body 1111 with a gate. After obtaining the amorphous alloy frame, it is only necessary to perform surface treatment in step S200 on the amorphous alloy frame to obtain the first frame 111. Compared with the second middle frame mentioned above, the processing time of the middle frame 1 can be effectively shortened, and the utilization rate of the material can be improved.

[0181] It should be noted that, in some embodiments, when manufacturing the middle frame 1 , an ingot made of a master alloy having the above raw materials may be directly die-cast to obtain an amorphous alloy frame.

[0182] Alternatively, see Fig. 9 As shown, in other embodiments, before the ingot is made into an amorphous alloy frame, the manufacturing method may further include:

[0183] Step S010: obtaining raw materials of master alloy;

[0184] Step S020: pre-melting at least part of the rare earth metal in the raw material and part of the zirconium element to obtain a pre-melted material;

[0185] Step S030: smelting the pre-melted material and the remaining raw materials obtained, and then pouring them after the smelting to obtain an ingot.

[0186] The raw materials of the master alloy can refer to the relevant description above, which will not be repeated here. By limiting the types of raw materials constituting the master alloy, an ingot containing the raw materials of the master alloy can be obtained after step S020 and step S030, so that a zirconium-based amorphous alloy frame with a tensile strength greater than 1400MPa can be obtained after die-casting the ingot.

[0187] The mass ratio of zirconium in step S020 and step S030 can be 1:9 to 9:1 to ensure that the rare earth metal can be better smelted with other raw materials. In the present application, the ratio of zirconium in step S020 and step S030 is not further limited.

[0188] It should be noted that since most rare earth metals have a high melting point, when the obtained rare earth metals include refractory rare earth metals with a relatively high melting point such as hafnium (Hf) and non-refractory rare earth metals with a relatively low melting point such as niobium (Nb), the refractory rare earth metals and part of the zirconium in the raw material can be pre-melted in step S020, and then the pre-melted material can be smelted with the non-refractory rare earth metals and other remaining raw materials.

[0189] Among them, refractory rare earth metals refer to rare earth metals with a melting point higher than 1650°C or higher than zirconium and with a certain reserve. The melting point of zirconium is 1852°C. Correspondingly, non-refractory rare earth metals refer to metals among rare earth metals with a melting point lower than that of refractory rare earth metals.

[0190] Alternatively, in some embodiments, if the obtained rare earth metals only include refractory rare earth metals such as hafnium (Hf), all the obtained rare earth metals and part of the zirconium in the raw material can be pre-melted in step S020. Correspondingly, if the obtained rare earth metals only include non-refractory rare earth metals such as niobium (Nb), step S020 can be omitted, and the obtained raw material can be directly smelted in step S030.

[0191] The pre-melting process in step S020 may be performed by electric arc or other methods.

[0192] The smelting process in step S030 includes vacuum induction melting process, the melting temperature of the vacuum induction melting process is 1900-2000°C, and the melting time is 5-10 minutes, so as to ensure that the pre-melted material and the remaining raw materials obtained can be fully melted at the above melting temperature and melting time for subsequent pouring.

[0193] In the present application, the melting temperature and melting time are not further limited. Generally, when the melting temperature is selected at a relatively low value within the above range, the melting time can be appropriately extended; or, when the melting temperature is selected at a relatively high value within the above range, the melting time can be appropriately shortened, as long as the pre-melted material and the remaining raw materials obtained can be fully melted.

[0194] It should be noted that after the smelting treatment, the temperature is lowered to the pouring temperature before pouring. The pouring temperature is 1200-1300°C so that an ingot can be obtained after pouring the master alloy after the smelting treatment. After the ingot is completely cooled in the pouring mold, it is taken out from the pouring mold. In this application, the shape of the pouring mold and the ingot is not further limited.

[0195] See also Fig.10 As shown, in step S200, the amorphous alloy frame is subjected to surface treatment, including:

[0196] Step S210: processing the amorphous alloy frame to obtain a rough blank of the frame body;

[0197] Step S220: forming a mirror surface on a part of the surface of the rough frame body to obtain the frame body;

[0198] Step S230: performing physical vapor deposition processing on the mirror surface to form a vapor deposition surface on the mirror surface of the frame body.

[0199] It should be noted that the structure of the frame body 1111 can refer to the relevant description above and will not be repeated here. After step S210 and step S220, a frame body 1111 with a mirror surface can be obtained, so that after the physical vapor deposition process in step S230, a vapor deposition layer 1114 can be formed on the mirror surface of the frame body, and the vapor deposition layer 1114 forms a vapor deposition surface 1115 on a side away from the first frame 111, so that the first frame 111 can have a mirror appearance texture at the vapor deposition surface 1115, thereby improving the appearance texture of the first frame 111.

[0200] The processing of the amorphous alloy frame in step S210 may include:

[0201] The gate on the amorphous alloy frame is removed by laser cutting, and the shape of the amorphous alloy frame is processed with high precision by CNC to ensure that the shape of the frame body 1111 meets the requirements.

[0202] In step S220, a part of the surface of the rough frame body can be polished to form a mirror surface. The structure of the frame body 1111 and the first frame 111 can be seen in Figure 5 shown.

[0203] When the frame 11 includes the second frame 112, the first frame 111 is disposed before the peripheral edge of the middle plate 12, and the manufacturing method further includes:

[0204] The second frame 112 is attached to the recessed area of ​​the first frame 111 . The recessed area is located on one side of the first frame 111 adjacent to the middle plate 12 and is annular. The density of the second frame 112 is less than that of the first frame 111 .

[0205] In this way, the recessed area is compensated by the second frame 112 , and the frame 11 and the middle frame 1 can be further reduced in weight without affecting the overall structure, strength, reliability of the middle frame 1 and the formation of the vapor deposition surface 1115 .

[0206] It should be noted that the number of the recessed areas, the locations of the recessed areas, and the molding material of the second frame 112 can be found in the above description, and will not be repeated here. Figure 7 shown.

[0207] The recessed area can be formed on the amorphous alloy frame during the die casting process of the ingot in the mold. Moreover, after the shape of the amorphous alloy frame at the recessed area is processed with high precision by CNC, it is beneficial to form the first frame 111 with the recessed area, so as to facilitate the fitting of the second frame 112.

[0208] The second frame 112 is attached to the recessed area of ​​the first frame 111, which may specifically include:

[0209] The second frame 112 is injection molded in the recessed area so that the second frame 112 and the first frame 111 form an integrated structure, thereby enhancing the connection strength between the second frame 112 and the first frame 111. The injection molding process may be nano injection molding or other injection molding methods for forming the second frame 112 in the recessed area. In this application, the specific method used in the injection molding process is not further limited. Nano injection molding is a common technology in the field of 3C products such as consumer electronics and communication products. In this application, the process of nano injection molding is not further limited.

[0210] The volume ratio of the second frame 112 in the frame 11 can be found in the relevant description above and will not be elaborated here.

[0211] It should be noted that, according to the design requirements of the middle frame 1, in some embodiments, after the second frame 112 is injection molded in the recessed area, the second frame 112 may be processed by CNC or other methods to obtain a middle frame 1 having a shape consistent with the design requirements. Therefore, in this application, the shape of the second frame 112 is not further limited.

[0212] The middle plate 12 can be made of lightweight metals such as aluminum alloy or magnesium alloy to increase the lightweight advantage of the middle frame 1. The metal middle plate can be made by die casting or profile plus CNC processing according to the structural design.

[0213] Depending on the material of the metal used for the middle plate 12, the method of anti-corrosion treatment on the surface of the middle plate 12 is different, so that the metal middle plate has a certain anti-corrosion performance. For example, when the middle plate 12 is made of die-cast or profile aluminum alloy, it can be anti-corrosion treated by anodizing, painting, etc. For another example, when the middle plate 12 is made of die-cast or profile magnesium alloy, it can be anti-corrosion treated by passivation, electrophoresis, micro-arc oxidation, painting, etc.

[0214] In step S300, the first frame 111 can be connected to the middle plate 12 through the connecting portion 1112 to realize the assembly of the frame 11 and the middle plate 12. The connection method of the connecting portion 1112 and the middle plate 12 can refer to the relevant description above, which will not be repeated here.

[0215] Below Figure 7 Taking the frame 11 in the figure as an example, and combining with specific embodiments, the manufacturing method of the middle frame 1 is further described.

[0216] Example 1

[0217] 1. Ingot production

[0218] Step S010: obtaining raw materials of master alloy;

[0219] The raw materials of the master alloy include Zr, Cu, Ni, Al, Fe and Hf, the molar fraction of Zr in the master alloy is 60, the molar fraction of Cu in the master alloy is 15.5, the molar fraction of Ni in the master alloy is 11, the molar fraction of Al in the master alloy is 12, the molar fraction of Fe in the master alloy is 1, and the molar fraction of Hf in the master alloy is 0.5;

[0220] Step S020: arc pre-melting the rare earth metal Hf element and part of the Zr element in the raw material to obtain a pre-melted material;

[0221] Step S030: smelting the pre-melted material and the remaining raw materials obtained, and then pouring them after the smelting to obtain an ingot.

[0222] Among them, pre-melting is arc pre-melting, and the smelting treatment is vacuum induction melting treatment. The melting temperature of vacuum induction melting treatment is 2000℃, and the melting time is 8min, to ensure that the pre-melted material and the remaining raw materials obtained are fully melted. After the melting treatment, the temperature is lowered to the pouring temperature for pouring. The pouring temperature is 1250℃, and the ingot is taken out after cooling to room temperature in the casting mold. The room temperature is generally 10-35℃, and the room temperature is also different depending on the environment. The ingot can be cooled to the room temperature of the current environment in the casting mold and taken out.

[0223] The mass ratio of zirconium element in step S020 and step S030 is 5:5.

[0224] 2. Making the First Border

[0225] Step S100: die-casting the ingot in a mold to obtain an amorphous alloy frame;

[0226] The die casting of the ingot in the mold specifically comprises the following steps:

[0227] melting the ingot at a first preset temperature;

[0228] After the ingot is melted, it is cooled to a second preset temperature and vacuum die-casted in a copper mold to obtain an amorphous alloy frame;

[0229] The first preset temperature is 1200°C, the second preset temperature is 800°C, and the vacuum degree of vacuum die casting is 10 - 2 The amorphous alloy frame is a zirconium-based amorphous alloy frame with a tensile strength greater than 1400 MPa. After vacuum die-casting, the amorphous alloy frame has two annular concave areas.

[0230] The zirconium-based amorphous alloy frame is made of Zr 60 Cu 15.5 Ni 11 Al 12 Fe1Hf 0.5 .

[0231] Step S200: performing surface treatment on the amorphous alloy frame to obtain a first frame;

[0232] The amorphous alloy frame is subjected to surface treatment, specifically comprising the following steps:

[0233] Step S210: processing the amorphous alloy frame to obtain a rough blank of the frame body;

[0234] Among them, the processing of the amorphous alloy frame includes using laser cutting to remove the gate on the amorphous alloy frame, and the shape of the amorphous alloy frame can be processed with high precision through CNC;

[0235] Step S220: forming a mirror surface on a part of the surface of the rough frame body to obtain the frame body;

[0236] In step S220, part of the surface of the rough frame body can be formed into a mirror surface by grinding and polishing;

[0237] Step S230: performing physical vapor deposition processing on the mirror surface to form a vapor deposition surface on the mirror surface of the frame body.

[0238] Due to the formation of the vapor deposition surface 1115, a mirror-like appearance can be obtained on the first frame 111. The vapor deposition surface 1115 is located on a surface of the first frame 111 away from the recessed area and forms the appearance surface of the first frame 111.

[0239] 3. The second frame fits the first frame

[0240] After mixing PC with 20% glass fiber, a second frame 112 is formed in the concave area of ​​the first frame 111 by nano injection molding to obtain a complete frame 11. 20% glass fiber means that the glass fiber accounts for 20% of the total mass of PC and glass fiber. The first frame 111 and the second frame 112 each account for half of the total volume of the frame 11.

[0241] 4. Production of medium plate

[0242] Firstly, a 6-series aluminum alloy extruded profile is selected and cut into a length suitable for the middle plate. Then, the 6-series aluminum alloy extruded profile is finely processed by CNC to obtain a middle plate rough blank. Finally, the surface of the middle plate rough blank is anodized to obtain the middle plate.

[0243] 5. Connection between the first frame and the middle plate

[0244] Step S300: a first frame is disposed around the peripheral edge of the middle plate and connected with the middle plate to form a middle frame, and the vapor deposition surface is the appearance surface of the middle frame.

[0245] The first frame 111 is connected to the metal middle plate via a glue structure.

[0246] The average density of the frame 11 of the middle frame 1 manufactured in Example 1 is 3.1 g / m 3 The tensile strength of the first frame 111 is greater than 1400 MPa, and the appearance surface has a mirror-like appearance texture.

[0247] Example 2

[0248] 1. Ingot production

[0249] Step S010: obtaining raw materials of master alloy;

[0250] The raw materials of the master alloy include Zr, Cu, Ni, Al, Nb and Hf, the molar fraction of Zr in the master alloy is 60, the molar fraction of Cu in the master alloy is 22, the molar fraction of Ni in the master alloy is 9, the molar fraction of Al in the master alloy is 3, the molar fraction of Nb in the master alloy is 5, and the molar fraction of Hf in the master alloy is 1;

[0251] Step S020: arc pre-melting the rare earth metal Hf element and part of the Zr element in the raw material to obtain a pre-melted material;

[0252] Step S030: smelting the pre-melted material and the remaining raw materials obtained, and then pouring them after the smelting to obtain an ingot.

[0253] Among them, the pre-melting is arc pre-melting, the smelting treatment is vacuum induction melting treatment, the melting temperature of vacuum induction melting treatment is 1950℃, and the melting time is 10min, so as to ensure that the pre-melted material and the remaining raw materials are fully melted. After the smelting treatment, the temperature is lowered to the pouring temperature for pouring, and the pouring temperature is 1250℃. After the ingot is cooled to the current room temperature in the casting mold, it is taken out.

[0254] The mass ratio of zirconium element in step S020 and step S030 is 6:5.

[0255] 2. Making the First Border

[0256] Step S100: die-casting the ingot in a mold to obtain an amorphous alloy frame;

[0257] The die casting of the ingot in the mold specifically comprises the following steps:

[0258] melting the ingot at a first preset temperature;

[0259] After the ingot is melted, it is cooled to a second preset temperature and vacuum die-casted in a copper mold to obtain an amorphous alloy frame;

[0260] The first preset temperature is 1150°C, the second preset temperature is 900°C, and the vacuum degree of vacuum die casting is 10 - 3 The amorphous alloy frame is a zirconium-based amorphous alloy frame with a tensile strength greater than 1400 MPa. After vacuum die-casting, the amorphous alloy frame has two annular concave areas.

[0261] The zirconium-based amorphous alloy frame is made of Zr 60 Cu 22 Ni9Al3Nb5Hf1.

[0262] Step S200: performing surface treatment on the amorphous alloy frame to obtain a first frame;

[0263] The amorphous alloy frame is subjected to surface treatment, specifically comprising the following steps:

[0264] Step S210: processing the amorphous alloy frame to obtain a rough blank of the frame body;

[0265] Among them, the processing of the amorphous alloy frame includes using laser cutting to remove the gate on the amorphous alloy frame, and the shape of the amorphous alloy frame can be processed with high precision through CNC;

[0266] Step S220: forming a mirror surface on a part of the surface of the rough frame body to obtain the frame body;

[0267] In step S220, part of the surface of the rough frame body can be formed into a mirror surface by grinding and polishing;

[0268] Step S230: performing physical vapor deposition processing on the mirror surface to form a vapor deposition surface on the mirror surface of the frame body.

[0269] Due to the formation of the vapor deposition surface 1115, a mirror-like appearance can be obtained on the first frame 111. The vapor deposition surface 1115 is located on a surface of the first frame 111 away from the recessed area and forms the appearance surface of the first frame 111.

[0270] 3. The second frame fits the first frame

[0271] After mixing PC with 20% glass fiber, a second frame 112 is formed in the concave area of ​​the first frame 111 by nano injection molding to obtain a complete frame 11. 20% glass fiber means that the glass fiber accounts for 20% of the total mass of PC and glass fiber. The first frame 111 and the second frame 112 each account for half of the total volume of the frame 11.

[0272] 4. Production of medium plate

[0273] Firstly, a die-casting magnesium alloy is selected, and Mg, Al, Zn, Mn and the like are melted and die-cast to obtain a middle plate die-casting. Then, the gate of the middle plate die-casting is removed by laser cutting, and then a local area of ​​the middle plate die-casting is fine-machined by CNC to obtain a middle plate rough blank. Finally, the surface of the middle plate rough blank is anodized to obtain the middle plate.

[0274] 5. Connection between the first frame and the middle plate

[0275] Step S300: a first frame is disposed around the peripheral edge of the middle plate and connected with the middle plate to form a middle frame, and the vapor deposition surface is the appearance surface of the middle frame.

[0276] The first frame 111 is connected to the metal middle plate via a glue structure.

[0277] The average density of the frame 11 of the middle frame 1 manufactured in Example 2 is 2.5 g / m 3 The tensile strength of the first frame 111 is greater than 1400 MPa, and the appearance surface has a mirror-like appearance texture.

[0278] On this basis, the embodiment of the present application provides two comparative examples, and tests or describes the average density and appearance texture of the middle frame in the two comparative examples, so as to compare with the middle frame of the present application. Among them, the first middle frame mentioned above can be regarded as comparative example 1, and the second middle frame can be regarded as comparative example 2.

[0279] The results show that the average density of the middle frame of Comparative Example 1 (first middle frame) is 7.9 g / m 3 The appearance surface has a mirror-like appearance texture. The appearance surface texture of the middle frame 1 manufactured in Example 1 and Example 2 is at least equivalent to the mirror-like appearance texture of the middle frame 1 of Comparative Example 2, and the average density of the middle frame 1 manufactured in Example 1 and Example 2 is much lower than the average density of the middle frame of Comparative Example 1. Therefore, compared with the middle frame 1 of Comparative Example 1, the middle frame 1 of the present application has a more obvious lightweight advantage.

[0280] The average density of the middle frame (second middle frame) of Comparative Example 2 is 2.7 g / m 3 The appearance surface is an anode appearance. The average density of the middle frame 1 manufactured in Example 1 and Example 2 is almost the same as the average density of the middle frame of Comparative Example 21. Therefore, the quality is also almost the same. The texture of the appearance surface of the middle frame 1 manufactured in Example 1 and Example 2 is much higher than that of the middle frame of Comparative Example 1.

[0281] It should be noted that the present application also provides a middle frame, which can be obtained by any of the above manufacturing methods. The structure of the obtained middle frame can refer to the above description of the structure of the middle frame 1, which will not be further elaborated here.

[0282] As described above, the electronic device 100 of the present application includes a display screen 3, a back cover 2 and the above-mentioned middle frame 1 or a middle frame manufactured by the above-mentioned manufacturing method. The middle frame 1 can be located between the display screen 3 and the back cover 2, and on the basis of providing stable support for the display screen 3 and the back cover 2, it can also enhance the appearance texture of the electronic device 100, which is conducive to realizing a lightweight design of the electronic device 100.

[0283] The assembly of the display screen 3 and the back cover 2 on the middle frame 1, as well as other structures of the electronic device 100 can be found in the relevant description above, and will not be repeated here.

[0284] In the description of the embodiments of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, or it can be an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to specific circumstances.

[0285] The terms "first", "second", "third", "fourth", etc. (if any) in the description and claims of the embodiments of the present application and the above-mentioned drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.

Claims

1. A middle frame, characterized in that: The invention comprises a frame and a middle plate, wherein the frame comprises a first frame connected to the middle plate, the first frame comprises a frame body, the molding material of the frame body comprises an amorphous alloy, and the frame body is arranged around the peripheral edge of the middle plate; a surface of the first frame away from the middle plate is a vapor deposition surface, the vapor deposition surface is a mirror surface, and the vapor deposition surface forms the appearance surface of the middle frame; The frame body comprises a connecting portion and an enclosing portion connected to each other, wherein the connecting portion is arranged around the peripheral edge of the middle plate and connected to the middle plate; The enclosing portion is arranged on a side of the connecting portion away from the middle plate, and forms a receiving space with the connecting portion and the middle plate; The first frame has at least one annular recessed area on one side adjacent to the middle plate, and the frame further includes a second frame matched with the shape of the recessed area, the second frame is accommodated in the recessed area and connected to the inner wall of the recessed area; the second frame is an injection molded part integrally connected to the first frame, and the molding material of the injection molded part includes plastic particles with a density lower than that of the amorphous alloy; The frame body of the first frame has an annular groove, which forms the recessed area, wherein along the thickness direction of the middle frame, the annular groove is distributed on at least one side of the middle plate and extends in a direction away from the middle plate.

2. The middle frame according to claim 1, characterized in that: The first frame further includes a vapor deposition layer, and a side of the frame body away from the middle plate is a mirror surface; the vapor deposition layer is deposited on the mirror surface of the frame body to form the vapor deposition surface on the first frame.

3. The middle frame according to claim 2, characterized in that: The frame body is a die-casting part of the amorphous alloy.

4. The middle frame according to claim 1, characterized in that: There are two annular grooves, which are distributed on opposite sides of the middle plate along the thickness direction of the middle frame and are symmetrically arranged on the frame body.

5. The middle frame according to claim 4, characterized in that: The bottom of the annular groove is a plane, and the side wall of the annular groove transitions to the bottom of the groove in an arc.

6. The middle frame according to claim 5, characterized in that: The thickness of the frame body at the bottom of the groove and the side wall adjacent to the middle plate is greater than or equal to 0.3 mm and less than or equal to 5 mm. The thickness of the frame body at the side wall away from the middle plate is greater than or equal to 0.15 mm.

7. The middle frame according to claim 5, characterized in that: The groove bottom and the side wall are connected by a rounded corner, and the radius of the rounded corner is greater than or equal to 0.2 mm.

8. The middle frame according to any one of claims 1 to 7, characterized in that: The second frame is located within the edge range of the first frame in the width direction of the middle plate, and the second frame and the middle plate together form a receiving space.

9. The middle frame according to claim 1, characterized in that: The plastic particles include at least one of polycarbonate, polyethylene and polystyrene.

10. The middle frame according to any one of claims 1 to 7, characterized in that: The volume ratio of the second frame to the frame is 1 / 2 to 2 / 3.

11. The middle frame according to any one of claims 1 to 7, characterized in that: The amorphous alloy includes a zirconium-based amorphous alloy.

12. The middle frame according to claim 11, characterized in that: The tensile strength of the first frame is greater than 1400 MPa.

13. A method for manufacturing a middle frame, characterized in that: The middle frame includes a frame and a middle plate, and the frame includes a first frame connected to the middle plate; the manufacturing method includes: Forming an ingot into an amorphous alloy frame, wherein the ingot is made of a master alloy; The amorphous alloy frame is surface-treated to obtain a first frame, one side of the first frame forms a vapor deposition surface, and the vapor deposition surface is a mirror surface; wherein the first frame includes a frame body, the frame body has an annular groove, the annular groove forms a recessed area, and along the thickness direction of the middle frame, the annular groove is distributed on at least one side of the middle plate and extends in a direction away from the middle plate; the frame body includes a connecting portion and an enclosing portion connected to each other, the connecting portion is arranged around the peripheral edge of the middle plate and connected to the middle plate; the enclosing portion is arranged around a side of the connecting portion away from the middle plate, and forms a receiving space with the connecting portion and the middle plate; Injection molding a second frame into the recessed area, wherein the density of the second frame is less than that of the first frame; The first frame is arranged around the peripheral edge of the middle plate and connected with the middle plate to form a middle frame, and the vapor deposition surface is the appearance surface of the middle frame.

14. The manufacturing method according to claim 13, characterized in that: The amorphous alloy frame includes a zirconium-based amorphous alloy frame.

15. The manufacturing method according to claim 14, characterized in that: The raw materials of the master alloy include zirconium, copper, nickel, aluminum and at least one rare earth metal.

16. The method according to any one of claims 13 to 15, characterized in that: The method of manufacturing the ingot into an amorphous alloy frame comprises: The ingot is die-casted in a mold to obtain the amorphous alloy frame, and the tensile strength of the amorphous alloy frame is greater than 1400 MPa.

17. The manufacturing method according to claim 16, characterized in that: The mold is a copper mold, and the ingot is die-casted in the mold, comprising: Melting the ingot at a first preset temperature; After the ingot is melted, the temperature is lowered to a second preset temperature, and vacuum die-casting is performed in the copper mold to obtain the amorphous alloy frame; The first preset temperature is greater than the melting point of the master alloy, the second preset temperature is greater than or equal to the melting point of the master alloy, and the vacuum degree of the vacuum die casting is 10 -2 ~10 -3 pa.

18. The manufacturing method according to claim 17, characterized in that: Before the ingot is made into an amorphous alloy frame, the manufacturing method further comprises: Obtaining raw materials for master alloy; Pre-melting at least a portion of the rare earth metal in the raw material and a portion of the zirconium element to obtain a pre-melted material; The premelt and the remaining raw materials are smelted, and then poured to obtain the ingot.

19. The manufacturing method according to claim 18, characterized in that: The smelting process includes vacuum induction smelting process, the smelting temperature of the vacuum induction smelting process is 1900-2000° C., and the smelting time is 5-10 minutes.

20. The method according to any one of claims 13 to 15, characterized in that: The surface treatment of the amorphous alloy frame comprises: Processing the amorphous alloy frame to obtain a frame body rough blank; Forming a mirror surface on part of the surface of the rough frame body to obtain the frame body; The mirror surface is subjected to physical vapor deposition treatment to form the vapor deposition surface on the mirror surface of the frame body.

21. A middle frame, characterized in that: The middle frame is obtained by the manufacturing method according to any one of claims 13-20.

22. An electronic device, characterized in that: It comprises a display screen, a back cover and a middle frame as claimed in claim 21 or a middle frame as claimed in any one of claims 1 to 12, wherein the middle frame is located between the display screen and the back cover.