A method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode

The three-dimensional polymer-carbon dot composite network is formed by using esterification and cross-linking reactions of long linear sodium alginate, calcium lignin sulfonate, graphitized carbon dots and silicon-based active substances in the silicon-based anode of lithium-ion batteries, and the solution is to solve the problem of esterification and cross-linking reactions of long linear sodium alginate, calcium lignin sulfonate, graphitized carbon dots and silicon-based active substances. The problem of insufficient conductivity and cycle stability of the silicon-based negative electrode is achieved, and the high-quality specific capacity and electrochemical activity are improved.

CN117727936BActive Publication Date: 2024-12-03HUNAN NORMAL UNIVERSITY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311766097.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-12-03
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

The prior art has shortcomings in improving the conductivity and cycle stability of the silicon-based anode of lithium-ion batteries, especially the mechanical strength, electronic conductivity/ionic conductivity, wetting and chemical stability are difficult to take into account, and the volume of the silicon-based anode during the cycle. The problems of expansion and lithium dendrites have not been effectively solved.

Method used

The moderate esterification and crosslinking reaction of long linear sodium alginate, calcium lignin sulfonate, graphitized carbon dots and silicon-based active substances is used to form a three-dimensional polymer-carbon dot composite network, and by absorbing a small amount of lithium salt electrolyte, it forms a Excellent gel electrolyte network, used in silicon-based anode, improving its electrochemical activity and stability.

Benefits of technology

The high-quality specific capacity, good electrochemical activity and stability of the semi-solid silicon negative electrode are achieved, and the cycle stability and rate performance of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117727936B_ABST
    Figure CN117727936B_ABST
Patent Text Reader

Abstract

The present invention is a method for preparing a carbon point enhanced gel electrolyte for a semi-solid silicon negative electrode, belonging to the technical field of lithium ion batteries, characterized in that sodium alginate and calcium lignin sulfonate are weighed in a mass ratio of (0.01-5): (0.01-2) and dissolved in deionized water for cross-linking reaction to form a glue solution, and then graphitized carbon points rich in hydroxyl and sulfonic acid functional groups are added to the glue solution to enhance cross-linking, and after stirring evenly, silicon-based active substances and conductive agents are added in sequence to obtain a slurry after stirring and coated on a copper foil, and moderately esterified and cross-linked in a vacuum oven to form a three-dimensional polymer-carbon point composite network and cut into circular pole pieces, and a gel electrolyte network with excellent electronic and lithium ion conductivity is obtained by absorbing 0.01-0.05mL of lithium salt electrolyte for silicon-based negative electrodes. The semi-solid silicon negative electrode disclosed in the present invention has both high ionic conductivity and excellent mechanical strength, and ultimately improves the electrochemical activity and cycle stability of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode. Background Art

[0002] The demand for upgrading automotive power batteries and large storage batteries has driven the development of high-energy lithium-ion batteries (LIBs). Silicon (Si)-based negative electrodes have become one of the key links in achieving high-energy lithium-ion batteries due to their ultra-high theoretical specific capacity, abundant reserves, and environmental friendliness. In particular, new polymer gel electrolytes have been introduced into silicon negative electrodes, and their good mechanical properties and electrical conductivity can effectively improve battery energy density, alleviate the volume expansion of silicon negative electrodes, inhibit the growth of lithium dendrites, maintain internal electrical contact and rate activity of electrodes, etc.

[0003] How to simultaneously take into account the processing performance, mechanical strength, electronic conductivity / ionic conductivity, wettability, and chemical stability of gel electrolytes is a very challenging and research-worthy study. To achieve the above goals, Jung et al. designed an esterified covalent bond between hydroxyl-rich graphene oxide and PAA to improve the conductive activity and suppress the volume strain of silicon (An in situformed graphene oxide-polyacrylic acid composite cage on silicon microparticles for lithium ion batteries via an esterification reaction, J. Mater. Chem. A, 2019, 7 (20), 12763-12772). Due to the lack of cross-linked structure, the mechanical strength of PAA is not enough to support the deep SOC and long cycle of silicon during the cycle process, and the graphene oxide is not uniformly dispersed, which makes the preset esterification reaction insufficient, and the cycle stability of the final silicon negative electrode is not significantly improved. The Chinese invention patent (publication number: CN112072106B) uses polyvinyl alcohol, sodium alginate and other polymers to obtain a polymerized polymer / amorphous carbon point mixed solution by hydrothermal treatment at 160-200°C, and mixes the solution with silicon nanomaterials to further coat it into a negative electrode sheet. Since the structure of the product obtained by hydrothermal treatment of polymers is often between polycondensates and amorphous carbon, that is, the product loses the viscosity unique to polymers, does not have the degree of graphitization that conductive carbon points should have, and its surface functional groups are even more uncontrollable, so this method has limited effect on improving the performance of silicon negative electrodes. In addition, the Chinese invention patent (publication number: CN110061239A) reported that lignin is used as the main body, and a small amount of inorganic sulfate and sodium alginate and other polymer additives are added in three steps to form a pre-polymerized lignin composite binder, which is finally processed with silicon powder materials to form a silicon negative electrode, and it is particularly emphasized that the first step of the prepolymerization reaction needs to be reacted at a constant temperature of 30-80°C in an inert gas atmosphere for 6-12 hours. Since this method uses lignin molecules with too short carbon chains as the main binder, the resulting polymer network has insufficient mechanical strength and elasticity, and no further monodisperse conductive carbon dots are added, the actual electrochemical activity and stability of the resulting silicon negative electrode do not reach the ideal state.

[0004] In summary, the present invention is designed to address the deficiencies of the above-mentioned technologies, and provides a method for preparing a carbon dot-enhanced gel electrolyte for a semi-solid silicon negative electrode. Its characteristics are: taking long straight-chain sodium alginate as the main body, a three-dimensional polymer-carbon dot composite network is formed based on the moderate esterification and cross-linking reaction between sodium alginate, calcium lignin sulfonate, graphitized carbon dots and silicon-based active substances, and finally a gel electrolyte network with excellent electronic and lithium ion conductivity is formed after absorbing a small amount of lithium salt electrolyte. Since the gel electrolyte network accounts for a small proportion in the silicon negative electrode structure and is integrally formed with the silicon powder material, the semi-solid silicon negative electrode finally formed has a high mass specific capacity, good electrochemical activity and stability. Summary of the invention

[0005] In view of the poor conductivity of silicon-based negative electrodes in lithium-ion batteries and the huge volume expansion during long cycles, the present invention provides a method for preparing a carbon dot-enhanced gel electrolyte for a semi-solid silicon negative electrode. To achieve the above-mentioned invention purpose, the technical solution of the present invention is to use long straight-chain sodium alginate as the main body, and to form a three-dimensional polymer-carbon dot composite network based on moderate esterification and cross-linking reactions between sodium alginate, calcium lignin sulfonate, graphitized carbon dots and silicon-based active substances. Then, by absorbing a small amount of lithium salt electrolyte, a gel electrolyte network with excellent electronic and lithium ion conductivity is obtained for the silicon-based negative electrode, which improves the cycle stability of the battery and has excellent rate performance.

[0006] A method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode, characterized in that it comprises the following steps:

[0007] ① Weigh 0.05-2 g of sodium alginate and calcium lignin sulfonate in a mass ratio of (0.01-5): (0.01-2) and dissolve them in 5 mL of deionized water. Control the temperature at 0°C to 30°C and stir to form glue solution A;

[0008] ② According to the mass ratio of sodium alginate and calcium lignin sulfonate: graphitized carbon dots (1-10): (0.1-1), carbon dots are weighed and added into the glue solution A obtained in step ①, and stirred for 0.5-2h to enhance crosslinking to obtain glue solution B;

[0009] ③ Add the silicon-based active material and the conductive agent to the glue obtained in step ② in sequence, and mix them evenly to form a slurry;

[0010] ④ The slurry is coated on the current collector copper foil, and moderately esterified and cross-linked in a vacuum oven to obtain a pole piece with a three-dimensional polymer-carbon dot composite network, and then the dried pole piece is taken out and cut into a circular pole piece with a slicer;

[0011] ⑤ Add 0.01-0.05 mL of lithium salt electrolyte to obtain a semi-solid silicon negative electrode with a gel electrolyte network;

[0012] The raw materials for preparing the graphitized carbon dots in step ② include one or more of graphite, acetylene black, lignin, glucose, citric acid, organic molecules of amino acids and biomass; the preparation method of the graphitized carbon dots includes high temperature pyrolysis, hydrothermal, microwave digestion, laser etching, strong acid oxidation, and electrolysis;

[0013] In step ③, the silicon-based active material is at least one of nano silicon powder, micro silicon powder, silicon-carbon composite material, and silicon oxide; the conductive agent is one or more of conductive carbon black, carbon nanotubes, carbon fiber, and graphene;

[0014] In step ③, the mass ratio of active material: conductive agent: glue is (60-95): (1-20):

[0015] (4~20);

[0016] The method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode is characterized in that: in step ④, the vacuum drying temperature is set to 50-200° C., and the vacuum drying time is 6-24 hours;

[0017] The method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode is characterized in that: in step ⑤, the operation of dripping 0.01 to 0.05 mL of electrolyte on a pole piece having a three-dimensional polymer-carbon dot composite network is carried out in a glove box, and the operating environment temperature is 0 to 40°C.

[0018] Technical Effects

[0019] The present invention has the following advantages:

[0020] 1. A semi-solid silicon negative electrode based on a three-dimensional polymer-carbon dot composite network was designed, and the conductivity of the material was improved through the three-dimensional conductive network covalent conductive structure.

[0021] 2. Graphitized carbon dots have abundant hydroxyl and sulfonic acid functional groups, which can enhance the mechanical properties of the semi-solid gel electrolyte network through intermolecular forces such as hydrogen bonds, while providing Lewis acid-base sites to promote the dissociation of lithium salts and provide more ion migration pathways, thereby improving the electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the XRD diagram of the semi-solid composite silicon negative electrode formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention, and the additive graphitized carbon dots.

[0023] Figure 2 This is a SEM image of a semi-solid composite silicon negative electrode formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention.

[0024] Figure 3 This is an XPS graph of the semi-solid composite silicon negative electrode Si 2p formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention.

[0025] Figure 4 This is the XPS graph of the semi-solid composite silicon negative electrode C1s formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention.

[0026] Figure 5 This is the XPS graph of the semi-solid composite silicon negative electrode S2p formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention.

[0027] Figure 6 This is the XPS graph of the semi-solid composite silicon negative electrode N1s formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention.

[0028] Figure 7 This is the FTIR graph of the semi-solid composite silicon negative electrode formed by cross-linking nano-silicon, sodium alginate, graphitized carbon dots, and calcium lignin sulfonate in Example 1 of the present invention, and the additive graphitized carbon dots.

[0029] Figure 8 This is a comparison chart of the cycle performance of button cells prepared based on the semi-solid silicon negative electrode with the addition of carbon dots in Example 1 of the present invention and the comparative example 1 without the addition of carbon dots.

[0030] Fig. 9 This is a comparison chart of the rate performance of button cells prepared based on the semi-solid silicon negative electrode with the addition of carbon dots in Example 1 of the present invention and the comparative example 1 without the addition of carbon dots.

[0031] Fig.10 This is a comparison chart of the AC impedance of the first cycle of charge and discharge of button batteries prepared based on the semi-solid silicon negative electrode with the addition of carbon dots in Example 1 of the present invention and the comparative example 1 without the addition of carbon dots.

[0032] Fig.11 This is a comparison chart of the AC impedance of the button-type batteries prepared based on the semi-solid silicon negative electrode with the addition of carbon dots in Example 1 of the present invention and the comparative example 1 without the addition of carbon dots at the 200th cycle of charge and discharge. DETAILED DESCRIPTION

[0033] The following examples are used to illustrate the present invention, but the embodiments of the present invention are not limited thereto, and are specifically carried out according to the following implementation methods:

[0034] Example 1

[0035] A carbon dot-enhanced gel electrolyte for a semi-solid silicon negative electrode is prepared by using calcium lignin sulfonate, sodium alginate, graphitized carbon dots, nano silicon powder and conductive carbon black.

[0036] (1) Preparation of graphitized carbon dots using acetylene black as raw material

[0037] First, measure 12mL H2SO4 and 4mL HNO 3, Then slowly add the concentrated sulfuric acid solution to the concentrated nitric acid solution and stir continuously. After cooling to room temperature, weigh 0.2g of acetylene black and add it to the prepared mixed acid solution in batches. After being dispersed evenly by ultrasonication for 30 minutes, put it into an oil bath pot and react at 85°C for 48 hours, and then cool to room temperature. Then neutralize it with Na2CO3 to a pH of 6-7, then use a centrifuge to centrifuge at 4000rpm for 10 minutes, and take the supernatant. Then dialyze and purify the solution at room temperature for 72 hours. After the dialysis is completed, freeze-drying is performed to obtain graphitized carbon dots with a particle size of about 2-10nm.

[0038] (2) Preparation of carbon dot-enhanced gel electrolyte for semi-solid silicon anode and battery assembly

[0039] First, weigh 0.1g sodium alginate and 0.015g calcium lignin sulfonate and add them into 5mL deionized water. -1 After 2 hours of magnetic stirring, a transparent glue A is formed, and then 0.06g of graphitized carbon dots are slowly added and stirred for 2 hours to crosslink to obtain glue B. Then 0.46g of nano silicon powder and 0.1g of conductive carbon black are added in batches and stirred for 1 hour to form a slurry. The slurry is coated on a copper foil with a 200um thickness applicator, and after drying, it is placed in a vacuum oven at 100°C for esterification and crosslinking to obtain a three-dimensional polymer-carbon dot composite network electrode. The dried electrode is taken out and cut into a circular electrode with a diameter of 12mm using a slicer. Subsequently, 0.03mL of lithium salt electrolyte is dripped on the electrode to obtain a semi-solid silicon negative electrode with a gel electrolyte network. Finally, in a glove box, a battery is assembled with a lithium sheet as the positive electrode and a celgard 2400 membrane as the diaphragm for electrochemical testing.

[0040] Example 2

[0041] A carbon dot-enhanced gel electrolyte for a semi-solid silicon negative electrode is prepared by using calcium lignin sulfonate, sodium alginate, graphitized carbon dots, nano silicon powder and conductive carbon black.

[0042] (1) Preparation of graphitized carbon dots using glucose as raw material

[0043] First, measure 12mL H2SO4 and 4mL HNO 3,Then slowly add the concentrated sulfuric acid solution into the concentrated nitric acid solution and stir continuously. After cooling to room temperature, weigh 0.4g of glucose and add it to the prepared mixed acid solution in batches. After being evenly dispersed by ultrasonication for 30 minutes, put it into an oil bath and react at 85°C for 48 hours, and then cool to room temperature. Then neutralize it with Na2CO3 to a pH of 6-7, then use a centrifuge to centrifuge at 4000rpm for 10 minutes, and take the supernatant. Then, dialyze the solution for purification at room temperature for 72 hours. After the dialysis is completed, freeze-dry it to obtain graphitized carbon dots with a particle size of about 2-10nm.

[0044] (2) Preparation of carbon dot-enhanced gel electrolyte for semi-solid silicon anode and battery assembly

[0045] First, weigh 0.1g sodium alginate and 0.01g calcium lignin sulfonate and add them into 5ml deionized water. -1 After 2 hours of magnetic stirring, a transparent glue A is formed, and then 0.03g of graphitized carbon dots are slowly added and stirred for 2 hours to crosslink to obtain glue B. Then 0.46g of micron silicon powder and 0.1g of conductive carbon black are added in batches and stirred for 1 hour to form a slurry. The slurry is coated on a copper foil with a 200um thickness applicator, and after drying, it is placed in a vacuum oven at 100°C for esterification and crosslinking to obtain a pole piece with a three-dimensional polymer-carbon dot composite network. The dried pole piece is then taken out and cut into a circular pole piece with a diameter of 12mm using a slicer. Subsequently, 0.05mL of lithium salt electrolyte is dripped on the pole piece to obtain a semi-solid silicon negative electrode with a gel electrolyte network. Finally, in a glove box, a battery is assembled with a lithium sheet as the positive electrode and a celgard 2400 membrane as the diaphragm for electrochemical testing.

[0046] Example 3

[0047] A carbon dot-enhanced gel electrolyte for a semi-solid silicon negative electrode is prepared by using calcium lignin sulfonate, sodium alginate, graphitized carbon dots, nano silicon powder and conductive carbon black.

[0048] (1) Preparation of graphitized carbon dots using amino acids as raw materials

[0049] First, measure 12mL H2SO4 and 4mL HNO 3,Then slowly add the concentrated sulfuric acid solution into the concentrated nitric acid solution and stir continuously. After cooling to room temperature, weigh 0.8g of amino acid and add it to the prepared mixed acid solution in batches. After being evenly dispersed by ultrasonication for 30 minutes, put it into an oil bath and react at 85°C for 48 hours, and then cool to room temperature. Then neutralize it with Na2CO3 to a pH of 6-7, then use a centrifuge to centrifuge at 4000rpm for 10 minutes, and take the supernatant. Then, dialyze the solution for purification at room temperature for 72 hours. After the dialysis is completed, freeze-dry it to obtain graphitized carbon dots with a particle size of about 2-10nm.

[0050] (2) Preparation of carbon dot-enhanced gel electrolyte for semi-solid silicon anode and battery assembly

[0051] First, weigh 0.1g sodium alginate and 0.02g calcium lignin sulfonate and add them into 5ml deionized water. -1 After 2 hours of magnetic stirring, a transparent glue A is formed, and then 0.1g of graphitized carbon dots is slowly added and stirred for 2 hours to crosslink to obtain glue B. Then 0.46g of silicon carbon powder and 0.1g of conductive carbon black are added in batches and stirred for 1 hour to form a slurry. The slurry is coated on a copper foil with a 200um thickness applicator, and after drying, it is placed in a vacuum oven at 100°C for esterification and crosslinking to obtain a three-dimensional polymer-carbon dot composite network electrode. The dried electrode is taken out and cut into a circular electrode with a diameter of 12mm using a slicer. Subsequently, 0.02mL of lithium salt electrolyte is dripped on the electrode to obtain a semi-solid silicon negative electrode with a gel electrolyte network. Finally, in a glove box, a battery is assembled with a lithium sheet as the positive electrode and a celgard 2400 membrane as the diaphragm for electrochemical testing.

[0052] Comparative Example 1

[0053] This comparative example is a gel electrolyte for a semi-solid silicon negative electrode without adding graphitized carbon dots, which is prepared by using calcium lignin sulfonate, sodium alginate, nano silicon powder and conductive carbon black.

[0054] (1) Preparation of gel electrolyte for semi-solid silicon anode and battery assembly

[0055] First, weigh 0.1g sodium alginate and 0.015g calcium lignin sulfonate and add them into 5mL deionized water. -1After 2 hours of magnetic stirring, a transparent glue A is formed. Then, 0.46g of nano silicon powder and 0.1g of conductive carbon black are added in batches and stirred for 1 hour to form a slurry. The slurry is coated on a copper foil with a 200um thick applicator, and after drying, it is placed in a vacuum oven at 100°C for esterification and cross-linking to obtain a three-dimensional polymer-carbon dot composite network electrode. The dried electrode is taken out and cut into a circular electrode with a diameter of 12mm using a slicer. Subsequently, 0.03mL of lithium salt electrolyte is dripped on the electrode to obtain a semi-solid silicon negative electrode with a gel electrolyte network. Finally, in a glove box, a battery is assembled with a lithium sheet as the positive electrode and a celgard 2400 membrane as the diaphragm for electrochemical testing.

[0056] Comparative Example 2

[0057] The silicon-based negative electrode is prepared by using sodium alginate, graphitized carbon dots, nano silicon powder and conductive carbon black.

[0058] (1) Preparation of graphitized carbon dots using acetylene black as raw material

[0059] First, measure 12mL H2SO4 and 4mL HNO 3, Then slowly add the concentrated sulfuric acid solution to the concentrated nitric acid solution and stir continuously. After cooling to room temperature, weigh 0.2g of acetylene black and add it to the prepared mixed acid solution in batches. After being dispersed evenly by ultrasonication for 30 minutes, put it into an oil bath pot and react at 85°C for 48 hours, and then cool to room temperature. Then neutralize it with Na2CO3 to a pH of 6-7, then use a centrifuge to centrifuge at 4000rpm for 10 minutes, and take the supernatant. Then dialyze and purify the solution at room temperature for 72 hours. After the dialysis is completed, freeze-drying is performed to obtain graphitized carbon dots with a particle size of about 2-10nm.

[0060] (2) Preparation of electrodes and assembly of batteries

[0061] First, weigh 0.1 g of sodium alginate and add it to 5 mL of deionized water. -1 After 2 hours of magnetic stirring, a transparent solution A is formed, and then 0.06g of graphitized carbon dots are slowly added and stirred for 2 hours to cross-link to obtain solution B. Then 0.46g of nano silicon powder and 0.1g of conductive carbon black are added in batches and stirred for 1 hour to form a slurry. The slurry is coated on the copper foil with a 75um thick applicator, and after drying, it is placed in a vacuum oven at 100°C, and then the dried electrode is taken out and cut into a circular electrode with a diameter of 12mm using a slicer. Then 0.05mL of lithium salt electrolyte is dripped on the electrode to obtain a negative electrode. Finally, in the glove box, a battery is assembled with a lithium sheet as the positive electrode and a celgard 2400 membrane as the diaphragm for electrochemical testing.

Claims

1. A method for preparing a carbon dot enhanced gel electrolyte for a semi-solid silicon negative electrode, characterized in that: The following steps are involved: ① Weigh 0.05-2 g of sodium alginate and calcium lignin sulfonate in a mass ratio of (0.01-5): (0.01-2) and dissolve them in 5 mL of deionized water. Control the temperature at 0°C to 30°C and stir to form glue solution A; ② According to the mass ratio of sodium alginate and calcium lignin sulfonate: graphitized carbon dots (1-10): (0.1-1), carbon dots are weighed and added into the glue solution A obtained in step ①, and stirred for 0.5-2h to enhance crosslinking to obtain glue solution B; ③ Add the silicon-based active material and the conductive agent to the glue obtained in step ② in sequence, and mix them evenly to form a slurry; ④ Coat the slurry on the current collector copper foil, moderately esterify and cross-link in a vacuum oven to obtain a three-dimensional polymer-carbon dot composite network electrode, then take out the dried electrode and cut it into round electrodes with a slicer; ⑤ Add 0.01-0.05 mL of lithium salt electrolyte to the electrode to prepare a semi-solid silicon negative electrode with a gel electrolyte network; The raw materials for preparing the graphitized carbon dots in step ② include one or more of graphite, acetylene black, lignin, glucose, and citric acid; the preparation method of the graphitized carbon dots includes high-temperature pyrolysis, hydrothermal, microwave digestion, laser etching, strong acid oxidation, and electrolysis; In step ③, the silicon-based active material is at least one of nano silicon powder, micro silicon powder, and silicon-carbon composite material; the conductive agent is one or more of conductive carbon black, carbon nanotubes, carbon fiber, and graphene; In the step ③, the mass ratio of active material: conductive agent: glue solution is (60-95): (1-20): (4-20).

2. The method for preparing the carbon dot enhanced gel electrolyte for semi-solid silicon negative electrode according to claim 1, characterized in that: In step ④, the vacuum drying temperature is set to 50-200° C., and the vacuum drying time is 6-24 hours.

3. The method for preparing the carbon dot enhanced gel electrolyte for semi-solid silicon negative electrode according to claim 1, characterized in that: In step ⑤, the operation of dripping 0.01-0.05 mL of lithium salt electrolyte onto the electrode is carried out in a glove box at an operating ambient temperature of 0-40°C.

Citation Information

Patent Citations

  • Lignin-based binder and preparation method thereof and lithium ion battery

    CN110061239A

  • A conductive binder material and its preparation method, a negative electrode sheet and a lithium-ion battery

    CN112072106B

  • High-performance cathode materials for lithium sulfur batteries from lignosulfonate

    CA2926796A1

  • Method for preparing silicon-based anode material adhesive of lithium ion battery

    CN103762367A

  • Preparation method of graphene quantum dot / nanometer silicon negative electrode material for lithium-ion battery