Nano-particle aluminum silicate fiber blanket and preparation method thereof

By uniformly spraying nanoparticle sol in the fiber blanket, spraying sealant and coating aluminum foil, the problems of uneven distribution of nanoparticles and easy shedding are solved, and the insulation performance and service life are significantly improved.

CN117734248BActive Publication Date: 2024-11-01SHANDONG GOLDEN ENERGY SAVING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311751696.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2024-11-01
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

The uneven distribution of nanoparticles in existing aerogel fiber blankets and easy to fall off, resulting in poor thermal insulation effect and service life.

Method used

The nanoparticle sol is uniformly sprayed into the fiber cotton by using the cotton collector process, and then sprayed with sealant and aluminum foil after needle-punching to form a sealing layer to enhance thermal insulation performance.

Benefits of technology

It achieves uniform distribution of nanoparticles inside and outside, enhances thermal insulation performance, avoids particulate matter falling off, and improves the service life and thermal insulation effect of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117734248B_ABST
    Figure CN117734248B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of refractory materials, and specifically relates to a nano-particle aluminum silicate fiber blanket and a preparation method thereof. The process includes the following steps: raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nano-particle sol → collecting cotton in a cotton collector → injecting nano-particle glue → needle punching into a blanket → spraying sealant on the surface → heat setting in a blanket heating furnace → aluminum foil coating → weighing and packaging; the cotton collecting process in the cotton collector sprays the nano-particle sol into the fiber cotton through a high-pressure nozzle, and the negative pressure circulating wind inside the cotton collector shell sucks the cotton, and the nano-particle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton mesh belt. The present invention provides a preparation method for integrally forming fiber cotton and additive nano-particle sol, which solves the problem of uneven distribution of the inner and outer layers of particles, excessive particles on the surface and easy to fall off, and enhances thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a nano-particle aluminum silicate fiber blanket and a preparation method thereof. Background Art

[0002] Aerogel fiber blankets are widely used in petrochemical pipeline insulation, metallurgical equipment energy-saving insulation, power pipeline insulation, LNG liquefaction pipeline cold insulation, and industrial furnace insulation and energy saving in various industries due to their excellent thermal insulation performance. The existing production process of aerogel fiber blankets is mostly carrier aluminum silicate fiber blanket production → nano raw material sol → gel → colloid infiltration or coating → high temperature curing sintering → finished product. Patent CN107415363A discloses a moisture-proof aluminum silicate fiber refractory felt, which is immersed in moisture-proof slurry and then dried, and then heat-resistant layers are connected on both sides, and then immersed in moisture-proof slurry again and dried. The moisture-proof slurry is made of Sargassum carbonized material, molecular sieve activation powder, and nano zirconium sol. This patent combines nanoparticles with aluminum silicate fiber felt by impregnation, which is easy to fall off in the later stage, affecting the thermal insulation effect and service life.

[0003] In the prior art, the nanoparticle coating method or the impregnation method results in uneven particles, which will lead to large deviations in the thermal conductivity of the fiber blanket. In addition, the particles on the surface of the fiber blanket prepared by this method are easy to fall off, which greatly affects the thermal insulation effect and service life of the aerogel fiber blanket. Therefore, there is an urgent need for a fiber blanket with good thermal insulation effect, uniform distribution of nanoparticles on the surface and inside and outside, and not easy to fall off, to solve the problems existing in the prior art. Summary of the invention

[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a nano-particle aluminum silicate fiber blanket, in which the nano-particle sol is evenly distributed inside and outside the fiber blanket, does not fall off, and has good thermal insulation performance.

[0005] The invention also provides a preparation method thereof, which is scientific, reasonable and suitable for large-scale production.

[0006] The method for preparing the nano-particle aluminum silicate fiber blanket of the present invention is characterized by comprising the following steps:

[0007] Raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nanoparticle sol → collecting cotton in cotton collector → injecting nanoparticles into glue → needle punching into blanket → spraying sealant on the surface → heat setting in blanket heating furnace → aluminum foil coating → weighing and packaging;

[0008] The cotton collector used in the cotton collecting process is provided with a cotton glue collector, which includes a plurality of high-pressure nozzles arranged on the side and top surfaces of the cotton collector housing, and a cotton mesh belt is arranged at the bottom of the cotton collector housing. The nanoparticle sol is sprayed into the fiber cotton through the high-pressure nozzles, and the negative pressure circulating wind inside the cotton collector housing sucks the cotton. The nanoparticle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton mesh belt. The structural schematic diagram of the cotton glue collector is shown in FIG. Figure 1 shown.

[0009] The raw materials are 45-55wt.% of aluminum oxide particles with a particle size of 200-300 meshes and 45-55wt.% of silicon oxide particles with a particle size of more than 200-300 meshes.

[0010] The temperature of the melting process is 2000-2300°C, and the spinning process for obtaining fiber cotton adopts three-roll spinning with a rotation speed of 13000-14000r / min.

[0011] The negative pressure of the cotton collector during the cotton collecting process is -0.8 to -0.7 MPa.

[0012] The injection amount of the nano-particle sol is 20-30% of the mass of the fiber cotton.

[0013] The nanoparticle sol is a mixture of component A, component B and an auxiliary agent in a mass ratio of 1:(0.8-1.2):(0.1-0.3); the raw materials of component A in the following mass fractions:

[0014] 1-3 parts of aluminum powder;

[0015] 1-3 parts of citric acid;

[0016] 10 parts water;

[0017] The B component has the following raw materials in parts by weight:

[0018] 2-3 parts of sodium silicate;

[0019] 1-2 parts of hydrochloric acid;

[0020] 10 parts water;

[0021] The auxiliary agent is a mixture of polyvinyl alcohol and isopropanol in a mass ratio of 1:(0.2-0.5);

[0022] The preparation method of the A component is to heat the raw material to 90-95°C and react for 5-6 hours to obtain the A component;

[0023] The preparation method of the B component is to heat the raw material to 60-65° C. and react for 5-6 hours to obtain the B component.

[0024] The needle punching blanket forming process adopts a double-sided needle punching machine, and the needle punching frequency is 100-120 times / min.

[0025] The temperature of the blanket heating furnace heat setting process is 550-680°C and the time is 40-50 minutes.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention provides a preparation method for integrally molding fiber cotton and additive nanoparticle sol, which solves the problem of uneven distribution of inner and outer layers of particles and excessive and easy-to-fall-off particles on the surface, thereby enhancing thermal insulation performance.

[0028] (2) After the fibers are needle-punched into a blanket, the present invention sets a production line spraying device to spray sealing glue on the blanket surface. After the blanket is put into a blanket heating furnace for curing and shaping, a first sealing layer for the nano powder particles is formed, and at the same time, the open pores on the surface of the fiber blanket are blocked to increase the thermal insulation performance.

[0029] (3) After the blanket is heat-set in a heating furnace, the fiber blanket is coated with aluminum foil to form a second seal for the nano-powder particles. At the same time, the reflective and refractive properties of the aluminum foil are utilized to further improve the thermal insulation performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a structural schematic diagram of the cotton cloth glue collecting device of the present invention;

[0031] in:

[0032] 1. High-pressure nozzle; 2. Cotton collector shell; 3. Cotton inlet; 4. Cotton mesh belt; 5. Cotton outlet. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto.

[0034] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0035] The sealant was purchased from Adhesive 1400 of Shandong Luyang Energy Saving Materials Co., Ltd.

[0036] The finished products prepared in the following examples and comparative examples are all fiber blankets with a thickness of 80 mm.

[0037] Example 1

[0038] The method for preparing the nano-particle aluminum silicate fiber blanket comprises the following steps:

[0039] Raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nanoparticle sol → collecting cotton in cotton collector → injecting nanoparticles into glue → needle punching into blanket → spraying sealant on the surface → heat setting in blanket heating furnace → aluminum foil coating → weighing and packaging;

[0040] The cotton collector used in the cotton collecting process is provided with a cotton collector and a glue distributing device, and the cotton collector and glue distributing device includes a plurality of high-pressure nozzles 1 arranged on the inner side and top surfaces of the cotton collector shell 2, and a cotton distributing mesh belt 4 is provided at the bottom of the cotton collector shell 2. The nano-particle sol is sprayed into the fiber cotton through the high-pressure nozzle 1, and the negative pressure circulating wind inside the cotton collector shell 2 sucks the cotton. The nano-particle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton distributing mesh belt 4, and the raw materials enter from the cotton inlet 3, and the finished products exit from the cotton outlet 5.

[0041] The raw materials are 45 wt.% of aluminum oxide particles with a particle size of 200-300 meshes and 55 wt.% of silicon oxide particles with a particle size of more than 200 meshes.

[0042] The temperature of the melting process is 2000°C, and the spinning process for obtaining fiber cotton adopts three-roll spinning with a rotation speed of 13000r / min.

[0043] The negative pressure of the cotton collector during the cotton collecting process is -0.8MPa.

[0044] The nanoparticle sol is a mixture of component A, component B and auxiliary agent in a mass ratio of 1:0.8:0.1; the raw materials of component A in the following mass fractions:

[0045] 1 part of aluminum powder;

[0046] 1 part citric acid;

[0047] 10 parts water;

[0048] The B component has the following raw materials in parts by weight:

[0049] 2 parts of sodium silicate;

[0050] 1 part hydrochloric acid;

[0051] 10 parts water;

[0052] The auxiliary agent is a mixture of polyvinyl alcohol and isopropanol in a mass ratio of 1:0.2;

[0053] The preparation method of the A component is to heat the raw material to 90°C and react for 6 hours to obtain the A component;

[0054] The preparation method of the B component is to heat the raw material to 60° C. and react for 6 hours to obtain the B component.

[0055] The injection amount of the nano-particle sol is 30% of the mass of the fiber cotton.

[0056] The needle punching blanket forming process adopts a double-sided needle punching machine with a needle punching frequency of 100 times / min.

[0057] The temperature of the blanket heating furnace heat setting process is 550° C. and the time is 50 minutes.

[0058] Example 2

[0059] The method for preparing the nano-particle aluminum silicate fiber blanket comprises the following steps:

[0060] Raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nanoparticle sol → collecting cotton in cotton collector → injecting nanoparticles into glue → needle punching into blanket → spraying sealant on the surface → heat setting in blanket heating furnace → aluminum foil coating → weighing and packaging;

[0061] The cotton collector used in the cotton collecting process is provided with a cotton collector and a glue distributing device, and the cotton collector and glue distributing device includes a plurality of high-pressure nozzles 1 arranged on the inner side and top surfaces of the cotton collector shell 2, and a cotton distributing mesh belt 4 is provided at the bottom of the cotton collector shell 2. The nano-particle sol is sprayed into the fiber cotton through the high-pressure nozzle 1, and the negative pressure circulating wind inside the cotton collector shell 2 sucks the cotton. The nano-particle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton distributing mesh belt 4, and the raw materials enter from the cotton inlet 3, and the finished products exit from the cotton outlet 5.

[0062] The raw materials are 55 wt.% of aluminum oxide particles with a particle size of 200-300 meshes and 45 wt.% of silicon oxide particles with a particle size of more than 300 meshes.

[0063] The temperature of the melting process is 2300°C, and the spinning process for obtaining fiber cotton adopts three-roll spinning with a rotation speed of 14000r / min.

[0064] The negative pressure of the cotton collector during the cotton collecting process is -0.7MPa.

[0065] The nanoparticle sol is a mixture of component A, component B and auxiliary agent in a mass ratio of 1:1.2:0.3; the raw materials of component A in the following mass fractions:

[0066] 3 parts of aluminum powder;

[0067] 3 parts of citric acid;

[0068] 10 parts water;

[0069] The B component has the following raw materials in parts by weight:

[0070] 3 parts of sodium silicate;

[0071] 2 parts hydrochloric acid;

[0072] 10 parts water;

[0073] The auxiliary agent is a mixture of polyvinyl alcohol and isopropanol in a mass ratio of 1:0.5;

[0074] The preparation method of the A component is to heat the raw material to 95°C and react for 5 hours to obtain the A component;

[0075] The preparation method of the B component is to heat the raw material to 65° C. and react for 5 hours to obtain the B component.

[0076] The injection amount of the nano-particle sol is 20% of the mass of the fiber cotton.

[0077] The needle punching blanket forming process adopts a double-sided needle punching machine with a needle punching frequency of 120 times / min.

[0078] The temperature of the blanket heating furnace heat setting process is 680° C. and the time is 40 minutes.

[0079] Example 3

[0080] The method for preparing the nano-particle aluminum silicate fiber blanket comprises the following steps:

[0081] Raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nanoparticle sol → collecting cotton in cotton collector → injecting nanoparticles into glue → needle punching into blanket → spraying sealant on the surface → heat setting in blanket heating furnace → aluminum foil coating → weighing and packaging;

[0082] The cotton collector used in the cotton collecting process is provided with a cotton collector and a glue distributing device, and the cotton collector and glue distributing device includes a plurality of high-pressure nozzles 1 arranged on the inner side and top surfaces of the cotton collector shell 2, and a cotton distributing mesh belt 4 is provided at the bottom of the cotton collector shell 2. The nano-particle sol is sprayed into the fiber cotton through the high-pressure nozzle 1, and the negative pressure circulating wind inside the cotton collector shell 2 sucks the cotton. The nano-particle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton distributing mesh belt 4, and the raw materials enter from the cotton inlet 3, and the finished products exit from the cotton outlet 5.

[0083] The raw materials are 50 wt.% of aluminum oxide particles with a particle size of 200-300 meshes and 50 wt.% of silicon oxide particles with a particle size of more than 250 meshes.

[0084] The temperature of the melting process is 2200°C, and the spinning process for obtaining fiber cotton adopts three-roll spinning with a rotation speed of 13000r / min.

[0085] The negative pressure of the cotton collector during the cotton collecting process is -0.8MPa.

[0086] The nanoparticle sol is a mixture of component A, component B and an auxiliary agent in a mass ratio of 1:1:0.2; the raw materials of component A in the following mass fractions:

[0087] 2 parts of aluminum powder;

[0088] 2 parts citric acid;

[0089] 10 parts water;

[0090] The B component has the following raw materials in parts by weight:

[0091] 2.5 parts of sodium silicate;

[0092] 1.5 parts of hydrochloric acid;

[0093] 10 parts water;

[0094] The auxiliary agent is a mixture of polyvinyl alcohol and isopropanol in a mass ratio of 1:0.3;

[0095] The preparation method of the A component is to heat the raw material to 90°C and react for 6 hours to obtain the A component;

[0096] The preparation method of the B component is to heat the raw material to 60° C. and react for 6 hours to obtain the B component.

[0097] The injection amount of the nano-particle sol is 25% of the mass of the fiber cotton.

[0098] The needle punching blanket forming process adopts a double-sided needle punching machine with a needle punching frequency of 110 times / min.

[0099] The temperature of the blanket heating furnace heat setting process is 600° C. and the time is 45 minutes.

[0100] Comparative Example 1

[0101] The same as Example 1, except that no aluminum foil coating is performed.

[0102] Comparative Example 2

[0103] The same as Example 1, except that the surface spraying of sealant and heat setting in a blanket heating furnace are not performed.

[0104] Fire resistance: The fire resistance of thermal insulation materials shall be tested in accordance with GB8624-2006.

[0105] Thermal conductivity: The thermal conductivity of the insulation material at 1200°C is tested in accordance with GB / T10294-2008.

[0106] The test data of Examples 1-3 and Comparative Examples 1-2 are shown in the following table:

[0107] Table 1 Test data

[0108]

[0109]

Claims

1. A method for preparing a nano-particle aluminum silicate fiber blanket, characterized in that: Including the following processes: Raw material feeding → melting → spinning into fibers to obtain fiber cotton → preparing nanoparticle sol → collecting cotton in cotton collector → injecting nanoparticles into glue → needle punching into blanket → spraying sealant on the surface → heat setting in blanket heating furnace → aluminum foil coating → weighing and packaging; The cotton collector used in the cotton collecting process is provided with a cotton collector and a glue collector, the cotton collector and glue collector comprises a plurality of high-pressure nozzles arranged on the side and top surfaces of the inner shell of the cotton collector, a cotton mesh belt is arranged at the bottom of the inner shell of the cotton collector, the nano-particle sol is sprayed into the fiber cotton through the high-pressure nozzle, the negative pressure circulating wind inside the cotton collector shell sucks the cotton, and the nano-particle sol and the fiber cotton are fully and evenly mixed and then fall onto the cotton mesh belt; The negative pressure of the cotton collector during the cotton collecting process is -0.8 to -0.7 MPa; The injection amount of the nanoparticle sol is 20-30% of the mass of the fiber cotton; The nanoparticle sol is a mixture of component A, component B and auxiliary agent in a mass ratio of 1:(0.8-1.2):(0.1-0.3); the component A is formed by the following raw materials in mass fractions: 1-3 parts of aluminum powder; 1-3 parts of citric acid; 10 parts water; The B component is formed by the following raw materials in parts by weight: 2-3 parts of sodium silicate; 1-2 parts of hydrochloric acid; 10 parts water; The auxiliary agent is a mixture of polyvinyl alcohol and isopropanol in a mass ratio of 1:(0.2-0.5); The preparation method of the A component is to heat the raw material to 90-95°C and react for 5-6 hours to obtain the A component; The preparation method of the B component is to heat the raw material to 60-65° C. and react for 5-6 hours to obtain the B component.

2. The method for preparing the nano-particle aluminum silicate fiber blanket according to claim 1, characterized in that: The nanoparticles in the nanoparticle sol are 45-55wt.% of aluminum oxide particles with a particle size of 200-300 meshes, and 45-55wt.% of silicon oxide particles with a particle size of more than 200-300 meshes.

3. The method for preparing the nano-particle aluminum silicate fiber blanket according to claim 1, characterized in that: The temperature of the melting process is 2000-2300°C, and the spinning process for obtaining fiber cotton adopts three-roll spinning with a rotation speed of 13000-14000r / min.

4. The method for preparing the nano-particle aluminum silicate fiber blanket according to claim 1, characterized in that: The needle punching blanket forming process adopts a double-sided needle punching machine, and the needle punching frequency is 100-120 times / min.

5. The method for preparing the nano-particle aluminum silicate fiber blanket according to claim 1, characterized in that: The temperature of the blanket heating furnace heat setting process is 550-680°C.

6. The method for preparing the nano-particle aluminum silicate fiber blanket according to claim 1, characterized in that: The time for the heat setting process in the blanket heating furnace is 40-50 minutes.

7. A nano-particle aluminum silicate fiber blanket, characterized in that: The nano-particle aluminum silicate fiber blanket is prepared by the preparation method of any one of claims 1 to 6.