A method for vanadium extraction from vanadium slag by calcium fixation
By adjusting the pH value in vanadium slag and performing oxidative roasting and acid leaching treatments, the problems of low vanadium conversion rate and viscous slurry in high-calcium vanadium slag were solved, achieving efficient vanadium extraction and improving the roasting-leaching rate and production efficiency of vanadium.
Patent Information
- Application Number
- CN202311588350.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-27
AI Technical Summary
In existing technologies, the vanadium conversion rate is low during the direct roasting-acid leaching process of high-calcium vanadium slag, and the large amount of calcium sulfate generated during the leaching process leads to a viscous slurry, making it difficult to effectively extract vanadium.
The pH of the vanadium slag system was adjusted to 2-3.5 using sulfuric acid for oxidative roasting and acid leaching. The liquid-solid ratio and pH value were controlled to prevent vanadium from combining with calcium and titanium to form insoluble vanadates, thereby reducing the liquid-solid ratio during acid leaching and improving the roasting-leaching efficiency of vanadium.
It significantly improves the vanadium roasting-leaching rate, avoids the formation of insoluble vanadates by combining vanadium with calcium and titanium during high-temperature roasting, reduces the viscosity of the slurry during acid leaching, and improves production efficiency.
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy smelting technology, specifically to a method for extracting vanadium from vanadium slag by solidifying calcium. Background Technology
[0002] Vanadium, as an important microalloying element, is widely used in metallurgy, chemical industry, aerospace and other fields. It can significantly improve the strength, toughness and ductility of steel, providing important support for ensuring the quality of key national projects. Vanadium-titanium magnetite is processed at high temperature in a blast furnace or electric furnace to obtain vanadium-containing molten iron. Vanadium slag is obtained by selective oxidation of the molten iron, which is used as a raw material for vanadium extraction.
[0003] With the rapid development of science and technology, high-quality steels such as low-temperature steel, marine steel, hydrogen-induced cracking resistant steel, and some thick plate steels require not only extremely low sulfur content but also phosphorus content ≤0.015%, 0.010%, or even 0.005%. To produce low-phosphorus steels, research has found that the converter vanadium extraction-steelmaking process can effectively remove phosphorus from vanadium-containing molten iron by adding lime, achieving simultaneous vanadium extraction and pre-dephosphorization, reducing the dephosphorization burden on the steelmaking process. However, the resulting vanadium slag shows an irreversible increasing Ca content, with CaO content reaching over 20% (i.e., high-calcium vanadium slag), far exceeding the level of existing vanadium slag.
[0004] Currently, the mainstream processes for vanadium extraction from vanadium slag are the sodium annealing method and the calcification method. In the sodium annealing roasting-water leaching process, CaO readily reacts with V₂O₅ to form water-insoluble calcium vanadate CaO·V₂O₅ or calcium-containing vanadium bronze CaV. 12 O 30 This significantly impacts the vanadium conversion rate during vanadium extraction. In the calcination-roasting-acid leaching process, high calcium content generates excessive calcium sulfate during wet acid leaching of vanadium, leading to a viscous leaching slurry that is difficult to stir and transport. Furthermore, during high-temperature roasting, excess calcium combines with titanium and iron in the vanadium slag to form vanadium-containing phases that are soluble in vanadates but difficult to dissolve in acid, drastically reducing the vanadium roasting conversion leaching rate.
[0005] Patent CN103397209B and patent document CN103397187A respectively add concentrated hydrochloric acid or concentrated nitric acid to the crushed high-calcium, high-phosphorus vanadium slag for activation treatment, so that calcium can be converted into calcium chloride / calcium nitrate, thereby achieving the purpose of decalcification. Then, the supernatant and low-calcium, low-phosphorus vanadium slag are obtained by filtration. The supernatant is then oxidized and precipitated, and evaporated and concentrated to obtain iron hydroxide and calcium chloride solids respectively. The low-calcium, low-phosphorus vanadium slag is used as vanadium extraction raw material for high-temperature calcification roasting-acid leaching vanadium extraction.
[0006] Patent CN112391537B discloses the following steps: 1. Coarsely crush and wet grind high-calcium, high-phosphorus vanadium slag to obtain filter residue with a particle size less than 0.175 mm; 2. Add water and hydrochloric acid to the filter residue, adjust the pH to 4-7, stir the reaction, filter and wash to obtain filter residue A; 3. Add a portion of filter residue A to sulfuric acid, adjust the pH to 0.1-0.8, react for 30-120 min, filter to obtain filtrate B and filter residue; 4. Add the remaining filter residue A to filtrate B, adjust the pH to 2-4, react for 30-120 min, filter to obtain filtrate C and filter residue D; 5. Add an extractant to filtrate C for extraction and back-extraction to obtain a vanadium-containing solution; 6. Roast and acid leach filter residue D to obtain a vanadium-containing leachate. This method has a long process, is complex, and is difficult to implement.
[0007] Patent CN111560523B describes a method for selective calcium leaching without additives – rapid and efficient calcium precipitation to prepare calcium carbonate – simple regeneration of the precipitation solution followed by non-replenishment leaching. The method primarily uses ammonium chloride solution for decalcification, and carbonate ions are added to the decalcification solution to precipitate calcium carbonate for reuse. This method is effective for removing dicalcium silicate from steel slag.
[0008] Patent CN112239808B describes a process where vanadium-containing, high-calcium, and high-phosphorus slag, after being crushed and wet-milled, is mixed with water. Sulfur dioxide gas is then introduced under stirring until the pH reaches 4-7, causing the calcium in the vanadium slag to form calcium bisulfite. The mixture is then filtered to obtain low-calcium vanadium-containing slag and a calcium-rich solution. The low-calcium vanadium-containing slag is roasted and acid-leached to extract vanadium, while the calcium-rich solution is heated to generate sulfur dioxide gas for reuse.
[0009] The existing technologies mainly involve decalcifying high-calcium vanadium slag to obtain low-calcium vanadium slag, and then extracting vanadium. However, the residual calcium in the vanadium slag after decalcification may combine to form insoluble compounds, reducing the vanadium yield. To address these issues, there is an urgent need to develop a method to further increase the vanadium yield. Summary of the Invention
[0010] The problem this invention aims to solve is the low vanadium conversion-leaching rate and the large amount of calcium sulfate generated during the leaching process of direct roasting-acid leaching of high-calcium vanadium slag, which leads to a viscous slurry.
[0011] The technical solution adopted in this invention is as follows:
[0012] The first aspect of this invention provides a method for extracting vanadium from vanadium slag by calcium fixation, comprising the following steps:
[0013] S1. Take the vanadium slag and add it to the solvent. Adjust the pH of the system to 2-3.5 with sulfuric acid. After the reaction, separate the solid and liquid components of the system to obtain vanadium slag A and solution A.
[0014] S2. Oxidize and roast vanadium slag A to obtain roasted material B;
[0015] S3. Acid leaching of roasted material B yields leachate B, which is then used as a raw material for vanadium extraction.
[0016] In this invention, after adjusting the pH of the system with sulfuric acid in step S1, the system pH is between 2 and 3.5, which ensures that calcium participates in the reaction completely. Although calcium in vanadium slag can react to form calcium sulfate in other pH ranges, such as when the system pH is 4, the system cannot guarantee that calcium in vanadium slag participates in the reaction completely in other pH ranges.
[0017] Preferably, the pH of the system in S1 includes, but is not limited to, 2.0, 2.5, 3 or 3.5.
[0018] Furthermore, by mass percentage, the vanadium slag contains more than 5% CaO and more than 2% V2O5.
[0019] Preferably, the vanadium slag contains more than 10% CaO.
[0020] More preferably, the vanadium slag contains more than 15% CaO.
[0021] Ordinary vanadium slag contains less than 3% calcium oxide. This invention targets high-calcium vanadium slag with more than 5% CaO, avoiding the formation of insoluble vanadates by the simultaneous combination of vanadium and calcium-titanium during the high-temperature roasting process of high-calcium vanadium slag. At the same time, the calcium in the vanadium slag no longer forms viscous calcium sulfate during the subsequent acid leaching process, which helps to reduce the liquid-solid ratio in the acid leaching process and improve the roasting-leaching efficiency of vanadium.
[0022] Furthermore, the liquid-to-solid ratio of the system in step S1 is 3–8:1 mL / g, and the reaction time is 20–60 min.
[0023] In some embodiments of the present invention, the liquid-to-solid ratio of the system in step S1 includes, but is not limited to, 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1, preferably 3 to 5:1.
[0024] Furthermore, the reaction step S1 also includes introducing oxygen into the system or adding hydrogen peroxide.
[0025] The purpose of introducing oxygen or adding hydrogen peroxide into the system is to reduce the iron content of solution A in step S1. Solution A after iron removal is easier to utilize in subsequent steps. In this invention, when the vanadium slag contains iron, in the system after pH adjustment with sulfuric acid in step S1, iron from the vanadium slag will enter the solution during the reaction (mainly ferrous iron). Adding air or hydrogen peroxide can oxidize the ferrous iron in the solution to ferric iron. Ferrous iron will begin to precipitate when the pH of the system reaches 1.8, and a large amount will precipitate above pH 3. This can better remove the iron from solution A, which is beneficial for the further utilization of solution A.
[0026] Furthermore, the solvent in step S1 is solution A and / or water.
[0027] Furthermore, step S3, acid leaching, includes:
[0028] S3-1 Take the roasted material B, add solvent and adjust it to make the liquid-solid ratio of the system 2-4:1mL / g and pH=2.5-3.5. Acid leaching for 30-60min, solid-liquid separation, to obtain residue B and leachate B;
[0029] Preferably, the liquid-to-solid ratio of the system includes, but is not limited to, 2:1 mL / g, 3:1 mL / g, 4:1 mL / g or 5:1 mL / g, and preferably, the pH of the system can be 2.3, 2.8, 3, 3.2 or 3.5.
[0030] S3-2 Take residue B, add solvent and adjust to make the system have a liquid-to-solid ratio of 1.2-3:1 mL / g and pH = 0.8-1.2. Acid leaching for 10-20 min, then adjust the pH of the system to 2.5-3.0, and separate the solid and liquid to obtain residue C and leachate C; preferably, the liquid-to-solid ratio of the system is including but not limited to 1.2:1 mL / g, 1.5:1 mL / g, 2:1 mL / g, and 3:1 mL / g; preferably, the pH of the system is including but not limited to 0.8, 1, or 1.2.
[0031] When the concentration of vanadium in leachate B is greater than 15 g / L, leachate B is used as a raw material for vanadium extraction.
[0032] When the vanadium concentration of leaching solution B is less than or equal to 15 g / L, leaching solution B is used as the solvent in step S3-1.
[0033] When the vanadium concentration in leaching solution C is greater than 3 g / L, leaching solution C is used as the solvent in step S3-1.
[0034] When the vanadium concentration in the leaching solution C is less than or equal to 3 g / L, the leaching solution C is used as the solvent in step S3-2.
[0035] When the concentration of vanadium in leachate B is less than 15 g / L, repeat steps S3-1 and S3-2 until the concentration of vanadium in leachate B is greater than 15 g / L, and then use leachate B as raw material for vanadium extraction.
[0036] The adjustment described in steps S3-1 and / or S3-2 is performed by adjusting with sulfuric acid.
[0037] The concentrations of vanadium in leachate B and leachate C in this invention are not limited to the aforementioned concentrations of 15 g / L and 3 g / L. The above concentrations are merely preferred concentration ranges applicable to this invention. The concentrations of vanadium in leachate B and leachate C in this invention can be adjusted according to the characteristics of the raw materials and the process. As long as the concentration of leachate B reaches the concentration required for vanadium extraction as a raw material, it is within the protection scope of this invention.
[0038] In this invention, the liquid-to-solid ratio of the S3-1 system is 2-4:1 mL / g. The acid-leaching roasted material B does not require a large liquid-to-solid ratio for leaching. This is because, during the acid leaching of vanadium slag in step S1, calcium in the vanadium slag reacts with sulfuric acid to form calcium sulfate dihydrate, which has a loose structure. After oxidation roasting in step S2, the water of crystallization in the calcium sulfate dihydrate disappears, and the crystal form inevitably changes. At this point, the acid-leaching roasted material B, with a liquid-to-solid ratio of 2-4:1 mL / g, allows a large amount of vanadium to enter the leaching solution B without causing problems such as viscous slurry or difficulty in stirring.
[0039] Furthermore, after adjusting the sulfuric acid system, if the pH of the system is lower than 2-3.5, an alkaline regulator is used to adjust the system. The alkaline regulator includes sodium hydroxide, ammonia, and / or calcium oxide, preferably ammonia.
[0040] Furthermore, the solvent in steps S3-1 and / or S3-2 also includes water.
[0041] Furthermore, the calcination conditions for step S2 are as follows: oxidative calcination at a temperature of 850–950°C for 30–90 minutes to obtain calcined material B.
[0042] Furthermore, the calcined material B undergoes a fine grinding step, with a fineness of 120 mesh or higher.
[0043] By adopting the above technical solution, the present invention has at least the following beneficial effects:
[0044] The present invention discloses a method for vanadium extraction from vanadium slag by fixing calcium. By adjusting the pH of the vanadium slag with sulfuric acid, excess calcium in the vanadium slag is converted into a highly stable phase. During the high-temperature oxidative roasting process, vanadium combines with the remaining calcium and manganese in the vanadium slag to form easily acid-soluble vanadates. This significantly avoids the formation of insoluble vanadates by combining vanadium with calcium and titanium during the high-temperature roasting process. At the same time, the calcium in the vanadium slag no longer forms viscous calcium sulfate during the subsequent acid leaching process, which helps to reduce the liquid-solid ratio in the acid leaching process and improve the roasting-leaching efficiency of vanadium.
[0045] In existing technologies, vanadium slag is typically directly roasted at high temperatures to obtain roasted feedstock, followed by acid leaching to extract vanadium. When the vanadium slag contains a high amount of calcium, the calcium reacts rapidly with sulfuric acid during the acid leaching process, generating a large amount of (dihydrate) calcium sulfate. This causes the slurry to gradually thicken, making stirring difficult and affecting vanadium leaching. Therefore, in this invention, the vanadium slag undergoes sulfuric acid leaching pretreatment. This serves two purposes: firstly, it avoids the formation of poorly soluble vanadates between vanadium and calcium titanium during high-temperature roasting, thus improving the vanadium leaching rate; secondly, it reduces the liquid-to-solid ratio in the vanadium extraction process, thereby increasing production efficiency. Detailed Implementation
[0046] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples.
[0047] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.
[0048] Unless otherwise defined, all scientific and technical terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art.
[0049] Unless otherwise specified, all percentages in this invention refer to mass percentages.
[0050] In this invention, the term "TV" refers to the total vanadium content, expressed as a percentage by mass, which includes V2O5.
[0051] In this invention, the term "high liquid-to-solid ratio" refers to a system with a liquid-to-solid ratio greater than 4:1 mL / g.
[0052] The beneficial effects of the present invention will be further illustrated below with reference to specific embodiments.
[0053] Example 1:
[0054] Take 120g of high-calcium vanadium slag (by mass percentage, CaO = 25.38%, TV = 5.85%) and add it to 600mL of water (liquid-solid ratio 5:1mL / g). Add sulfuric acid under stirring to control the pH at 2.5-3.0. After reacting for 40min, separate the solid and liquid to obtain vanadium slag A (dry weight 138.9g, TV = 4.72%).
[0055] Take 130g of vanadium slag A and calcine it at 900℃ for 60min to obtain 117.4g of calcined material B (TV=5.23%). Grind the calcined material to 120 mesh.
[0056] Take 100g of finely ground roasted material B, add it to 250mL of water for acid leaching, use sulfuric acid to control the pH to 3.0, react for 60min, and then separate the solid and liquid to obtain residue B (dry weight 85.3g, TV = 0.82%) and vanadium-containing leachate B (vanadium content = 18.8g / L). The vanadium leaching rate here is 86.61%.
[0057] Take 50g of residue B and add it to 100mL of water for acid leaching (liquid-solid ratio 2:1mL / g). Use sulfuric acid to control the pH at 1.5. After reacting for 20min, use ammonia to adjust the pH of the system to 3.0. Separate the solid and liquid to obtain residue C (dry weight 42.5g, TV = 0.62%) and vanadium-containing leachate C (vanadium content = 1.46g / L). The vanadium leaching rate here is 35.73%.
[0058] Vanadium-containing leachate B is used as a raw material to prepare qualified vanadium oxide products using conventional vanadium precipitation methods. Vanadium-containing leachate C is returned to be used as an acid leaching solvent for residue B.
[0059] In this embodiment, the high-calcium vanadium slag is first treated with sulfuric acid, and then roasted and acid-leached, with a total vanadium dissolution rate of 91.39% in the roasted material.
[0060] Example 2:
[0061] Take 150g of high-calcium vanadium slag (by mass percentage, CaO = 18.76%, TV = 8.42%), add it to 450mL of water (liquid-solid ratio 3:1mL / g), add sulfuric acid under stirring to control the pH at 3.0-3.5, and after reacting for 60min, separate the solid and liquid to obtain vanadium slag A (dry weight 175.3g, TV = 7.16%).
[0062] Take 150g of vanadium slag A and roast it at 880℃ for 30min to obtain 140.8g of roasted material B (TV=7.63%). Grind the roasted material to -120 mesh.
[0063] Take 120g of finely ground roasted material B, add it to 360mL of water for acid leaching, use sulfuric acid to control the pH to 2.8, react for 45min, and then separate the solid and liquid to obtain residue B (dry weight 93.2g, TV = 1.20%) and vanadium-containing leachate B (vanadium content = 22.2g / L). The vanadium leaching rate here is 87.79%.
[0064] Take 100g of residue B and add it to 200mL of water for acid leaching. Use sulfuric acid to control the pH at 1.0. After reacting for 20min, adjust the pH of the system to 2.5 using lime milk. Separate the solid and liquid to obtain residue C (dry weight 92.3g, TV = 0.43%) and vanadium-containing leachate C (vanadium content = 4.02g / L). The vanadium leaching rate here is 66.92%.
[0065] Vanadium-containing leachate B is used as a raw material to prepare qualified vanadium oxide products using conventional vanadium precipitation methods. Vanadium-containing leachate C is returned to the roasting process and used as an acid leaching solvent for roasting material B.
[0066] In this Example 2, the total vanadium dissolution rate was 95.96%.
[0067] Comparative Example 1: (Vanadium extraction by direct high-temperature roasting and acid leaching)
[0068] Take 300g of high-calcium vanadium slag (by mass percentage, CaO = 25.38%, TV = 5.85%), oxidize and roast at 900℃ for 30min to obtain 301.1g of roasted material (TV = 5.83%), and grind the roasted material to -120 mesh.
[0069] Take 100g of roasted material and add it to 250mL of water for acid leaching (initial pH of the system = 8.86). Use sulfuric acid to control the pH of the system to 3.0. During this process, when the pH gradually drops from 8.86 to 3.0, a large amount of calcium sulfate is produced in the system, the slurry gradually becomes viscous, stirring becomes difficult, and acid leaching cannot continue.
[0070] Take another 100g of roasted material and add it to 1050mL of water. Under this liquid-solid ratio, acid leaching is carried out, with the pH controlled at 3.0 using sulfuric acid. The reaction is carried out for 60min, and the solid and liquid are separated to obtain residue B' (dry weight 154.7g, TV = 1.45%) and vanadium-containing leachate B' (vanadium content = 6.2g / L). The vanadium leaching rate here is 74.44%.
[0071] 100g of residue B' was added to 200mL of water for acid leaching, followed by solid-liquid separation. The pH was controlled at 1.5 using sulfuric acid, and the reaction was carried out for 20 minutes. The pH was then adjusted to 3.0 using ammonia, and solid-liquid separation was performed again, yielding residue C' (dry weight 97.4g, TV = 0.95%) and vanadium-containing leachate C' (vanadium content = 1.9g / L). The vanadium leaching rate was 36.19%.
[0072] In Comparative Example 1, the vanadium slag was directly roasted and acid leached, and the total vanadium dissolution rate was 83.69%.
[0073] In Comparative Example 1, by mass percentage, the aforementioned high-calcium vanadium slag direct roasting material containing 25.38% CaO was acid-leached at a liquid-solid ratio of 2.5:1 mL / g. The slurry was viscous and difficult to stir, making it impossible to continue acid leaching. The liquid-solid ratio had to be increased to 7:1 mL / g for normal stirring, but the vanadium concentration of the resulting leachate was much lower than that in Example 1.
[0074] Comparative Example 2: (Vanadium extraction by direct high-temperature roasting and acid leaching)
[0075] Take 150g of high-calcium vanadium slag (by mass percentage, CaO = 18.76%, TV = 8.42%), oxidize and roast at 880℃ for 60min to obtain 159.7g of roasted material (TV = 7.91%), and grind the roasted material to 120 mesh.
[0076] Take 120g of roasted material and add it to 360mL of water (initial pH of the system = 8.45). Use sulfuric acid to control the pH of the system to 2.8. During this process, when the pH gradually drops from 8.45 to 2.8, a large amount of calcium sulfate is produced in the system, the slurry gradually becomes viscous, stirring becomes difficult, and acid leaching cannot continue.
[0077] Take another 120g of roasted material and add it to 720mL of water. Under this liquid-solid ratio, acid leaching is carried out, with the pH controlled at 2.8 using sulfuric acid. The reaction is carried out for 45min, and the solid and liquid are separated to obtain residue B (dry weight 108.8g, TV = 1.64%) and vanadium-containing leachate B (vanadium content = 10.60g / L). The vanadium leaching rate here is 81.20%.
[0078] Take 100g of residue B” and add it to 300mL of water for acid leaching. Separate the solid and liquid components, control the pH to 1.0 with sulfuric acid, react for 20min, and adjust the pH of the system to 2.5 with lime milk to obtain residue C” (dry weight 98.9g, TV = 0.94%) and vanadium-containing leachate C” (vanadium content = 2.29g / L). The vanadium leaching rate here is 43.3%.
[0079] In Comparative Example 2, the vanadium slag was directly roasted and acid leached, and the total vanadium leaching rate was 89.34%.
[0080] In Comparative Example 2, when the 18.76% high-calcium slag direct roasting material was acid leached at a liquid-solid ratio of 3:1 mL / g, the slurry also showed problems of viscosity and difficulty in stirring. It was necessary to increase the liquid-solid ratio to 6:1 mL / g to achieve normal stirring, but the vanadium concentration of the resulting leachate was much lower than that in Example 2.
[0081] It should be noted that the components or steps in the above embodiments can be interchanged, substituted, added, or deleted. Therefore, the combinations formed by these reasonable permutations and transformations should also fall within the protection scope of this invention, and the protection scope of this invention should not be limited to the above embodiments.
[0082] The above are exemplary embodiments disclosed in this invention. The order of the disclosed embodiments is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. However, it should be noted that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of this invention (including the claims) is limited to these examples. Various changes and modifications can be made without departing from the scope defined by the claims. The functions, steps, and / or actions of the methods according to the disclosed embodiments described herein do not need to be performed in any particular order. Furthermore, although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular.
[0083] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method for extracting vanadium from vanadium slag by calcium fixation, characterized in that, Includes the following steps: S1. Add vanadium slag to a solvent, adjust the pH of the system to 2-3.5 with sulfuric acid, and after the reaction, separate the solid and liquid components of the system to obtain vanadium slag A and solution A; S2. Oxidize and roast vanadium slag A to obtain roasted material B; S3. Acid leaching of roasted material B yields leachate B, which is then used as a raw material for vanadium extraction. By mass percentage, the vanadium slag contains more than 5% CaO and more than 2% V2O5; The liquid-to-solid ratio of the S1 system is 3~8:1 mL / g, and the reaction time is 20~60 min; S1 also includes the introduction of oxygen into the system or the addition of hydrogen peroxide; S3 acid leaching includes: S3-1 Take roasted material B, add solvent and adjust it to make the liquid-solid ratio of the system 2-4:1mL / g, pH=2.5-3.5, acid leaching for 30-60min, solid-liquid separation, to obtain residue B and leachate B; S3-2 Take residue B, add solvent and adjust it so that the system is at a liquid-to-solid ratio of 1.2-3:1 mL / g and pH=0.8-1.
2. Acid leaching for 10-20 min, then adjust the pH of the system to 2.5-3.0, and separate the solid and liquid to obtain residue C and leachate C; When the concentration of vanadium in leachate B is greater than 15 g / L, leachate B is used as a raw material for vanadium extraction. When the vanadium concentration in leachate B is less than or equal to 15 g / L, leachate B is used as the solvent in S3-1. When the vanadium concentration in leachate C is greater than 3 g / L, leachate C is used as the solvent in S3-1. When the vanadium concentration in leachate C is less than or equal to 3 g / L, leachate C is used as the solvent for S3-2. The S2 calcination conditions are: oxidative calcination at 850~950℃ for 30~90min to obtain calcined material B.
2. The method as described in claim 1, characterized in that, The solvent for S1 is solution A and / or water.
3. The method as described in claim 1, characterized in that, After adjusting the system with sulfuric acid, if the pH of the system is lower than 2-3.5, an alkaline regulator is used to adjust the system. The alkaline regulator includes one or more of sodium hydroxide, ammonia, and calcium oxide.
4. The method according to any one of claims 1 to 3, characterized in that, The solvent in S3-1 and / or S3-2 also includes water.
5. The method as described in claim 1, characterized in that, The roasted material B undergoes a fine grinding process, with a fineness of ≥120 mesh.
Citation Information
Patent Citations
Method for vanadium extraction by activating high-calcium high-phosphorus vanadium slag with nitric acid
CN103397187A
Method for extracting vanadium from high-calcium and high-phosphorus vanadium slag
CN103397209B
A method for vanadium extraction from vanadium-containing, high-calcium, and high-phosphorus slag
CN112239808B
A method for vanadium extraction using hydrochloric acid, sulfuric acid, and vanadium-containing high-calcium and high-phosphorus slag.
CN112391537B
Method of extraction of vanadium from high- calcium slags
RU2160786C1