A method for preparing lightweight aluminum single panels
By using specific aluminum alloy formulations and processes, the problem of uneven recrystallization in lightweight aluminum panels was solved, resulting in refined grains and improved film bonding strength, thereby enhancing the overall performance and corrosion resistance of the aluminum panels.
Patent Information
- Application Number
- CN202311819764.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-27
AI Technical Summary
In the recrystallization annealing process of existing lightweight aluminum panels, the precipitation of supersaturated solid solutions and the inhomogeneity of the microstructure lead to inconsistent recrystallization in alloy regions, affecting surface gloss and mechanical properties.
By employing specific aluminum alloy formulations and processes, including melting, refining, purification, cold rolling, annealing, and surface treatment, the recrystallized grains are refined, and homogenization pretreatment and surface treatment are performed to improve the film bonding strength.
This method achieves a uniform and fine grain structure in aluminum alloy sheets, increases the cube texture content and corrosion resistance of the film, and enhances the overall performance of the sheet and the bonding strength between the film and the substrate.
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum panel manufacturing technology, and in particular to a method for manufacturing lightweight aluminum panels. Background Technology
[0002] In industry, aluminum composite panels used in building materials often employ 3-series Al-Mn alloys, which are non-heat-treatable wrought aluminum alloys. These materials possess excellent comprehensive properties, including light weight, moderate strength, high plasticity, good ductility and workability, good weldability, strong corrosion resistance, and a smooth surface. A representative example is the 3003 Al-Mn alloy, which, due to the addition of Mn, has higher strength and hardness than pure aluminum and is widely used in containers, decorative building materials, and other applications.
[0003] In existing lightweight aluminum panels, the precipitation of supersaturated solid solutions and the inhomogeneity of the microstructure during subsequent recrystallization annealing will lead to inconsistent recrystallization processes in some areas of the alloy, resulting in coarse and uneven recrystallized grains. If the alloy sheet in this state continues to undergo subsequent finishing processes, it will result in a rough and dull surface, and its mechanical properties will be difficult to meet requirements. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing lightweight aluminum single-panel, thereby solving the problems in the above-mentioned background technical solutions.
[0005] The above-mentioned technical objective of the present invention is achieved through the following technical solution: A method for preparing lightweight aluminum single-layer panels, characterized by comprising the following steps: S1, pure aluminum ingots, aluminum-manganese master alloy, iron agent, silicon agent, copper agent, and refining agent are mixed according to the mixing ratio; S2, first put the pure aluminum ingot into the smelting furnace and smelt it in the temperature range of 740~760℃. After the aluminum liquid is completely melted, the remaining materials are added and smelted. S3, the slag removal process is carried out on the molten metal; S4, the molten metal is transferred to a holding furnace for secondary refining, which uses powder spraying refining and argon refining. S5 involves adding titanium wire to molten metal, followed by purification through a degassing box and a filtration box. S6, the purified molten metal enters the front box with the temperature controlled at 690~705℃, and the molten metal discharged from the front box enters the casting nozzle for dispersion. Then, after passing through the inclined casting and rolling mill, it is rolled into an aluminum alloy plate with a casting and rolling speed of 900~1000mm / min. S7, the aluminum alloy plate is subjected to homogenization pretreatment annealing at annealing temperatures of 520℃, 540℃, 560℃, 580℃ and 600℃ for 22 hours. S8, the pre-treated annealed aluminum alloy sheet is placed on a four-roll irreversible rolling mill for cold rolling; S9, followed by recrystallization annealing, which is carried out in a muffle furnace, with the annealing regime being held at 360℃, 380℃, and 400℃ for 3 hours; S10: First, the aluminum alloy plate is sanded with sandpaper and then cleaned and dried with deionized water. After sanding, the aluminum alloy plate is immersed in alkaline etching solution for alkaline etching. After alkaline etching, it is cleaned and dried with deionized water. Then, it is immersed in pickling solution at room temperature for pickling. After pickling, it is rinsed and dried with deionized water to complete the pretreatment. S11, the pre-treated aluminum alloy plate is immersed in the conversion treatment solution for chemical conversion treatment, and then dried to obtain the surface-treated aluminum alloy plate. S12 involves coating the surface-treated aluminum alloy sheet with primer and topcoat sequentially via roller coating, baking and flattening it, and then applying a film to obtain a lightweight aluminum single panel.
[0006] Preferably, in step S2, titanium dioxide needs to be coated on the inner wall of the smelting furnace when the preheating temperature reaches 300°C.
[0007] Preferably, in step S2, after the aluminum liquid has completely melted, hexachloroethane is added first for degassing.
[0008] Preferably, the actual composition of the aluminum alloy plate in S6 is controlled as follows: Si is 0.2%~0.4%, Fe is 0.4%~0.6%, Cu is 0.10%~0.16%, Mn is 1.10%~1.20%, Mg is 0~0.05%, and the balance is Al.
[0009] Preferably, the specific cold rolling process in S8 is as follows: the rolling is completed in 5 passes, the final thickness after rolling is 1 mm, the rolling speed is 850 m / min, the total reduction rate of all passes is 85.3%~88.1%, and the average reduction rate of each pass is 33%~35%.
[0010] Preferably, the specific method of sanding in S10 is as follows: use three grades of sandpaper, namely 400#, 800#, and 1000#, to sand away the natural layer on the surface of the aluminum alloy plate in turn.
[0011] Preferably, the alkaline etching solution in S10 is at 45~50℃, the alkaline etching time is 3min, and the alkaline etching solution includes 2~5g / L NaOH and 20~40g / L Na2CO3.
[0012] Preferably, the pickling solution in S10 includes 50~90 ml / L of HNO3 and 1~5 ml / L of CH3COOH, and the pickling time is 1 min.
[0013] Preferably, the conversion treatment solution in S11 comprises the following components: 5 g / L K2ZrF6, 5 g / L NaVO3, 4 g / L NaF, and 2 g / L TBHP.
[0014] In summary, the present invention has the following beneficial effects: In this invention, the grain size of the aluminum alloy sheet after pre-annealing is significantly reduced after final annealing. The sheet after pre-annealing not only obtains a relatively uniform and fine grain structure, but also increases the content of cubic texture.
[0015] This invention refines recrystallized grains and improves the uniformity of the overall microstructure and the content of cube texture by increasing the cold rolling deformation and final annealing temperature. These two factors promote recrystallization before precipitation, minimize the interaction between precipitation and recrystallization during annealing, reduce the influence of precipitation on recrystallization nucleation, and increase the cold rolling deformation to increase the probability of particle nucleation, effectively reducing the recrystallization activation energy.
[0016] This invention removes residual impurities from the surface of the aluminum alloy plate after grinding by alkaline etching, and accelerates deposition by exposing the cathode point of the substrate, thereby accelerating film formation or increasing film thickness. Furthermore, the final pickling treatment can improve the bonding strength between the subsequent film layer and the substrate.
[0017] The conversion film on the aluminum alloy plate after subsequent surface treatment of the present invention has good corrosion resistance and higher bonding strength with the substrate. Detailed Implementation
[0018] The specific embodiments of the present invention will be further described below. These embodiments do not constitute a limitation on the present invention. Example 1
[0019] A method for preparing lightweight aluminum single-layer panels includes the following steps: S1, pure aluminum ingots, aluminum-manganese master alloy, iron agent, silicon agent, copper agent, and refining agent are mixed according to the mixing ratio; S2. When the preheating temperature of the smelting furnace reaches 300℃, titanium dioxide needs to be coated on the inner wall of the smelting furnace. Pure aluminum ingots are first put into the smelting furnace and smelted at a temperature of 740℃. After the aluminum liquid is completely melted, hexachloroethane is first added for degassing, and then the remaining materials are added for smelting. S3, the slag removal process is carried out on the molten metal; S4, the molten metal is transferred to a holding furnace for secondary refining, which uses powder spraying refining and argon refining. S5 involves adding titanium wire to molten metal, followed by purification through a degassing box and a filtration box. S6. The purified molten metal enters the front chamber, where the temperature is controlled at 690℃. The molten metal discharged from the front chamber enters the casting nozzle for dispersion, and then passes through an inclined casting and rolling mill to roll out an aluminum alloy plate. The actual composition of the aluminum alloy plate is controlled as follows: Si 0.2%~0.4%, Fe 0.4%~0.6%, Cu 0.10%~0.16%, Mn 1.10%~1.20%, Mg 0~0.05%, with the balance being Al. The casting and rolling speed used is 900mm / min. S7, the aluminum alloy plate is subjected to homogenization pretreatment annealing at annealing temperatures of 520℃, 540℃, 560℃, 580℃ and 600℃ for 22 hours. S8 involves placing the pre-annealed aluminum alloy sheet on a four-high irreversible rolling mill for cold rolling, specifically in five passes, resulting in a final thickness of 1 mm. The rolling speed is 850 m / min, the total reduction rate for all passes is 85.3%, and the average reduction rate for each pass is 33%~35%. S9, followed by recrystallization annealing, which is carried out in a muffle furnace, with the annealing regime being held at 360℃, 380℃, and 400℃ for 3 hours; S10: First, use three layers of sandpaper (400#, 800#, and 1000#) to grind and remove the natural layer on the surface of the aluminum alloy plate. Then, clean and dry it with deionized water. After grinding, immerse the aluminum alloy plate in an alkaline etching solution for alkaline etching. After alkaline etching, clean and dry it with deionized water. Then, immerse it in an acid pickling solution at room temperature for acid pickling. After acid pickling, rinse and dry it with deionized water to complete the pretreatment. S11, the pre-treated aluminum alloy plate is immersed in the conversion treatment solution for chemical conversion treatment, and then dried to obtain the surface-treated aluminum alloy plate. S12 involves coating the surface-treated aluminum alloy sheet with primer and topcoat sequentially via roller coating, baking and flattening it, and then applying a film to obtain a lightweight aluminum single panel.
[0020] The alkaline etching solution was prepared at 45°C for 3 minutes. The alkaline etching solution consisted of 2 g / L NaOH and 20 g / L Na2CO3.
[0021] The pickling solution consists of 50 ml / L HNO3 and 1 ml / L CH3COOH, and the pickling time is 1 min.
[0022] The conversion treatment solution comprises the following components: 5 g / L K2ZrF6, 5 g / L NaVO3, 4 g / L NaF, and 2 g / L TBHP. Example 2
[0023] A method for preparing lightweight aluminum single-layer panels includes the following steps: S1, pure aluminum ingots, aluminum-manganese master alloy, iron agent, silicon agent, copper agent, and refining agent are mixed according to the mixing ratio; S2. When the preheating temperature of the smelting furnace reaches 300℃, titanium dioxide needs to be coated on the inner wall of the smelting furnace. Pure aluminum ingots are first put into the smelting furnace and smelted in a temperature range of 750℃. After the aluminum liquid is completely melted, hexachloroethane is first added for degassing, and then the remaining materials are added for smelting. S3, the slag removal process is carried out on the molten metal; S4, the molten metal is transferred to a holding furnace for secondary refining, which uses powder spraying refining and argon refining. S5 involves adding titanium wire to molten metal, followed by purification through a degassing box and a filtration box. S6, the purified molten metal enters the front chamber with the temperature controlled at 700℃. The molten metal discharged from the front chamber enters the casting nozzle for dispersion, and then passes through the inclined casting and rolling mill to roll out aluminum alloy plates. The actual composition of the aluminum alloy plates is controlled as follows: Si is 0.2%~0.4%, Fe is 0.4%~0.6%, Cu is 0.10%~0.16%, Mn is 1.10%~1.20%, Mg is 0~0.05%, and the balance is Al. The casting and rolling speed is 950mm / min. S7, the aluminum alloy plate is subjected to homogenization pretreatment annealing at annealing temperatures of 520℃, 540℃, 560℃, 580℃ and 600℃ for 22 hours. S8 involves placing the pre-annealed aluminum alloy sheet on a four-high irreversible rolling mill for cold rolling, specifically in five passes, resulting in a final thickness of 1 mm. The rolling speed is 850 m / min, with a total reduction of 86.7% across all passes and an average reduction of 33% to 35% per pass. S9, followed by recrystallization annealing, which is carried out in a muffle furnace, with the annealing regime being held at 360℃, 380℃, and 400℃ for 3 hours; S10: First, use three layers of sandpaper (400#, 800#, and 1000#) to grind and remove the natural layer on the surface of the aluminum alloy plate. Then, clean and dry it with deionized water. After grinding, immerse the aluminum alloy plate in an alkaline etching solution for alkaline etching. After alkaline etching, clean and dry it with deionized water. Then, immerse it in an acid pickling solution at room temperature for acid pickling. After acid pickling, rinse and dry it with deionized water to complete the pretreatment. S11, the pre-treated aluminum alloy plate is immersed in the conversion treatment solution for chemical conversion treatment, and then dried to obtain the surface-treated aluminum alloy plate. S12 involves coating the surface-treated aluminum alloy sheet with primer and topcoat sequentially via roller coating, baking and flattening it, and then applying a film to obtain a lightweight aluminum single panel.
[0024] The alkaline etching solution was set at 47°C for 3 minutes. The alkaline etching solution consisted of 4 g / L NaOH and 30 g / L Na2CO3.
[0025] The pickling solution consists of 70 ml / L HNO3 and 3 ml / L CH3COOH, and the pickling time is 1 min.
[0026] The conversion treatment solution comprises the following components: 5 g / L K2ZrF6, 5 g / L NaVO3, 4 g / L NaF, and 2 g / L TBHP. Example 3
[0027] A method for preparing lightweight aluminum single-layer panels includes the following steps: S1, pure aluminum ingots, aluminum-manganese master alloy, iron agent, silicon agent, copper agent, and refining agent are mixed according to the mixing ratio; S2. When the preheating temperature of the smelting furnace reaches 300℃, titanium dioxide needs to be coated on the inner wall of the smelting furnace. Pure aluminum ingots are first put into the smelting furnace and smelted in a temperature range of 760℃. After the aluminum liquid is completely melted, hexachloroethane is first added for degassing, and then the remaining materials are added for smelting. S3, the slag removal process is carried out on the molten metal; S4, the molten metal is transferred to a holding furnace for secondary refining, which uses powder spraying refining and argon refining. S5 involves adding titanium wire to molten metal, followed by purification through a degassing box and a filtration box. S6. The purified molten metal enters the front chamber, where the temperature is controlled at 705℃. The molten metal discharged from the front chamber enters the casting nozzle for dispersion, and then passes through an inclined casting and rolling mill to roll out an aluminum alloy plate. The actual composition of the aluminum alloy plate is controlled as follows: Si 0.2%~0.4%, Fe 0.4%~0.6%, Cu 0.10%~0.16%, Mn 1.10%~1.20%, Mg 0~0.05%, with the balance being Al. The casting and rolling speed is 1000mm / min. S7, the aluminum alloy plate is subjected to homogenization pretreatment annealing at annealing temperatures of 520℃, 540℃, 560℃, 580℃ and 600℃ for 22 hours. S8 involves placing the pre-annealed aluminum alloy sheet on a four-high irreversible rolling mill for cold rolling, specifically in five passes, resulting in a final thickness of 1 mm. The rolling speed is 850 m / min, with a total reduction rate of 88.1% across all passes and an average reduction rate of 33% to 35% per pass. S9, followed by recrystallization annealing, which is carried out in a muffle furnace, with the annealing regime being held at 360℃, 380℃, and 400℃ for 3 hours; S10: First, use three layers of sandpaper (400#, 800#, and 1000#) to grind and remove the natural layer on the surface of the aluminum alloy plate. Then, clean and dry it with deionized water. After grinding, immerse the aluminum alloy plate in an alkaline etching solution for alkaline etching. After alkaline etching, clean and dry it with deionized water. Then, immerse it in an acid pickling solution at room temperature for acid pickling. After acid pickling, rinse and dry it with deionized water to complete the pretreatment. S11, the pre-treated aluminum alloy plate is immersed in the conversion treatment solution for chemical conversion treatment, and then dried to obtain the surface-treated aluminum alloy plate. S12 involves coating the surface-treated aluminum alloy sheet with primer and topcoat sequentially via roller coating, baking and flattening it, and then applying a film to obtain a lightweight aluminum single panel.
[0028] The alkaline etching solution was set at 50°C for 3 minutes. The alkaline etching solution consisted of 5 g / L NaOH and 40 g / L Na2CO3.
[0029] The pickling solution consists of 90 ml / L HNO3 and 5 ml / L CH3COOH, and the pickling time is 1 min.
[0030] The conversion treatment solution comprises the following components: 5 g / L K2ZrF6, 5 g / L NaVO3, 4 g / L NaF, and 2 g / L TBHP.
[0031] The performance of the aluminum single-layer panels prepared in the above embodiments and ordinary fluorocarbon aluminum single-layer panels on the market were tested according to the national standard GB / T23443~2009 as comparative example 1. The test results are shown in Table 1.
[0032] Table 1 Performance test data of aluminum single-panel samples from various embodiments sample Pencil hardness / H Peel strength (N / mm) Abrasion resistance (L / μm) Chemical corrosion resistance Impact resistance Example 1 2 0.43 6.8 No change No cracks Example 2 2 0.48 6.7 No change No cracks Example 3 2 0.43 6.8 No change No cracks Comparative Example 1 1 0.18 5.3 No change There are cracks As can be seen from Table 1, the lightweight aluminum single panel prepared by this invention not only meets national standards, but also has good strength and hardness, and stronger chemical corrosion resistance.
[0033] In this invention, the grain size of the aluminum alloy sheet after pre-annealing is significantly reduced after final annealing. The sheet after pre-annealing not only obtains a relatively uniform and fine grain structure, but also increases the content of cubic texture.
[0034] This invention refines recrystallized grains and improves the uniformity of the overall microstructure and the content of cube texture by increasing the cold rolling deformation and final annealing temperature. These two factors promote recrystallization before precipitation, minimize the interaction between precipitation and recrystallization during annealing, reduce the influence of precipitation on recrystallization nucleation, and increase the cold rolling deformation to increase the probability of particle nucleation, effectively reducing the recrystallization activation energy.
[0035] This invention removes residual impurities from the surface of the aluminum alloy plate after grinding by alkaline etching, and accelerates deposition by exposing the cathode point of the substrate, thereby accelerating film formation or increasing film thickness. Furthermore, the final pickling treatment can improve the bonding strength between the subsequent film layer and the substrate.
[0036] The conversion film on the aluminum alloy plate after subsequent surface treatment of the present invention has good corrosion resistance and higher bonding strength with the substrate.
[0037] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art can make various modifications or equivalent substitutions to the present invention within the scope of its essence and protection. Such modifications or equivalent substitutions should also be considered to fall within the protection scope of the present invention.
Claims
1. A method for preparing lightweight aluminum single-layer panels, characterized in that, Includes the following steps: S1, pure aluminum ingots, aluminum-manganese master alloy, iron agent, silicon agent, copper agent, and refining agent are mixed according to the mixing ratio; S2, first put the pure aluminum ingot into the smelting furnace and smelt it in the temperature range of 740~760℃. After the aluminum liquid is completely melted, the remaining materials are added and smelted. S3, the slag removal process is carried out on the molten metal; S4, the molten metal is transferred to a holding furnace for secondary refining, which uses powder spraying refining and argon refining. S5 involves adding titanium wire to molten metal, followed by purification through a degassing box and a filtration box. S6, the purified molten metal enters the front box with the temperature controlled at 690~705℃, and the molten metal discharged from the front box enters the casting nozzle for dispersion. Then, after passing through the inclined casting and rolling mill, it is rolled into an aluminum alloy plate with a casting and rolling speed of 900~1000mm / min. S7, the aluminum alloy plate is subjected to homogenization pretreatment annealing at annealing temperatures of 520℃, 540℃, 560℃, 580℃ and 600℃ for 22 hours. S8 involves placing the pre-annealed aluminum alloy sheet on a four-high irreversible rolling mill for cold rolling in five passes, resulting in a final thickness of 1 mm. The rolling speed is 850 m / min, with a total reduction rate of 85.3% to 88.1% across all passes and an average reduction rate of 33% to 35% per pass. S9, followed by recrystallization annealing, which is carried out in a muffle furnace, with the annealing regime being held at 360℃, 380℃, and 400℃ for 3 hours; S10: First, the aluminum alloy plate is sanded with sandpaper and then cleaned and dried with deionized water. After sanding, the aluminum alloy plate is immersed in alkaline etching solution for alkaline etching. After alkaline etching, it is cleaned and dried with deionized water. Then, it is immersed in pickling solution at room temperature for pickling. After pickling, it is rinsed and dried with deionized water to complete the pretreatment. S11, the pretreated aluminum alloy plate is immersed in the conversion treatment solution for chemical conversion treatment, and then dried to obtain the surface-treated aluminum alloy plate. The conversion treatment solution includes the following components: 5 g / L K2ZrF6, 5 g / L NaVO3, 4 g / L NaF, and 2 g / L TBHP. S12, after surface treatment, the aluminum alloy plate is coated with primer and topcoat in sequence by roller coating, baked and flattened, and then laminated to obtain lightweight aluminum single panel. The actual composition of the aluminum alloy plate in S6 is controlled as follows: Si is 0.2%~0.4%, Fe is 0.4%~0.6%, Cu is 0.10%~0.16%, Mn is 1.10%~1.20%, Mg is 0~0.05%, and the balance is Al.
2. The method for preparing a lightweight aluminum single panel according to claim 1, characterized in that: When the preheating temperature of the S2 furnace reaches 300°C, titanium dioxide needs to be coated on the inner wall of the furnace.
3. The method for preparing a lightweight aluminum single panel according to claim 1, characterized in that: After the aluminum liquid in S2 has completely melted, hexachloroethane is first added for degassing.
4. The method for preparing a lightweight aluminum single panel according to claim 1, characterized in that: The specific method for sanding in S10 is as follows: use three grades of sandpaper, 400#, 800#, and 1000#, to sand away the natural layer on the surface of the aluminum alloy plate in turn.
5. The method for preparing a lightweight aluminum single panel according to claim 1, characterized in that: The alkaline etching solution in S10 is at 45~50℃ and the alkaline etching time is 3min. The alkaline etching solution includes 2~5g / L NaOH and 20~40g / L Na2CO3.
6. The method for preparing a lightweight aluminum single panel according to claim 1, characterized in that: The pickling solution in S10 consists of 50-90 ml / L of HNO3 and 1-5 ml / L of CH3COOH, and the pickling time is 1 min.
Citation Information
Patent Citations
Manufacturing method of high-elongation aluminum alloy strip for battery shell
CN107419140A
Environment-friendly chemical conversion processing technology for aluminum alloy
CN109652790A