A method for treating cold-heading steel without adding aluminum slag

By alloying followed by slag washing in the cold heading steel process, combined with argon stirring and alloy control, the problem of large amounts of flue gas caused by the use of aluminum slag was solved, achieving environmental protection and quality assurance in aluminum slag-free smelting.

CN117737564BActive Publication Date: 2026-11-10SGIS SONGSHAN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311645967.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2026-11-10
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Existing cold heading steel processing methods using aluminum slag produce large amounts of flue gas, making it difficult to meet environmental protection requirements.

Method used

When the steel is tapped from the converter, high manganese and aluminum-iron are added first for alloying, and then lime is added for slag washing. After the molten steel is sampled at the argon station, the amount of aluminum wire fed is increased according to the acid-soluble aluminum content. After the LF furnace, lime, fluorite and synthetic slag are added to control the acid-soluble aluminum content of the molten steel, and it is treated by argon stirring and calcium wire feeding.

Benefits of technology

The absence of aluminum slag during the smelting process significantly reduces flue gas generation, avoids dust pollution, and ensures the quality of molten steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for treating cold-heading steel without adding aluminum slag, belonging to the field of metallurgical technology. The method includes the following steps: When tapping steel from the converter, high manganese and ferroaluminum are first added for alloying, followed by lime for slag washing; samples are taken at the argon station, and the amount of aluminum wire fed is increased based on the acid-soluble aluminum content in the steel; after the steel reaches the LF furnace, lime, fluorite, and synthetic slag are added, and argon gas is passed through under power supply for stirring. The argon gas is then reduced, and a first sample is taken, observing the slag color. After the first sample is obtained, aluminum wire is fed and lime is added again based on the acid-soluble aluminum composition of the steel and the color of the refining slag. Argon gas is passed through for stirring, and a second sample is taken. The acid-soluble aluminum content of the steel is controlled at 0.030%-0.035%, the silicon content at 0.03%-0.06%, and the sulfur content <0.007%. Calcium wire is fed for soft blowing, completing the LF furnace refining process. Through these steps, aluminum slag can be avoided, dust generation is prevented, and the quality of the molten steel is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical technology, and more specifically, to a method for treating cold-headed steel without adding aluminum slag. Background Technology

[0002] The chemical composition of SWRCH22A cold-heading steel smelted by Shaogang Steel is as follows: carbon 0.20-0.22%, silicon less than 0.06%, manganese 0.75-0.85%, phosphorus less than 0.02%, sulfur less than 0.012%, and acid-soluble aluminum 0.020-0.045%. The original technology involved tapping the steel in the converter using 40 cubic meters per hour of argon gas. When the steel was tapped to 1 / 3 capacity, 500 kg of lime, 100 kg of aluminum slag, 1050 kg of high-manganese steel, and 350 kg of ferroaluminum were added in sequence. After tapping, the steel was purged with 40-60 cubic meters per hour of argon gas for 3-5 minutes, then the argon gas was turned off and a sample was taken at the argon station. After the sample was obtained, the argon gas was turned on again, and aluminum wire was fed to adjust the acid-soluble aluminum content in the molten steel to 0.025%-0.050%. If it was higher than 0.050%, [further action was taken]. Then, no additional aluminum wire is needed. After the molten steel reaches the LF furnace, add 350 kg of lime, 500 kg of synthetic slag, and 100 kg of aluminum slag. After energizing for 8-15 minutes, take sample one. Based on the acid-soluble aluminum content of the steel sample, feed aluminum wire to a concentration of 0.070%-0.080%, while simultaneously adding other alloys. Stir with 60-100 cubic meters / hour of argon gas for 3-5 minutes. Reduce the argon gas flow and take sample two. Based on the acid-soluble aluminum content of sample two, adjust the concentration to 0.040%-0.048%. After feeding the aluminum wire, use 15-20 cubic meters / hour of argon gas for 5 minutes, then measure the temperature and raise it to the outlet temperature +15℃. Feed in 160-200 meters of calcium wire and use 5-15 cubic meters / hour of argon gas for a soft blowing process for 12-20 minutes before exiting the station.

[0003] The original technology for treating cold-headed steel is relatively mature and the quality is relatively stable, but it produces a lot of smoke when aluminum slag is added, which does not meet environmental protection requirements.

[0004] Therefore, this invention is proposed. Summary of the Invention

[0005] The purpose of this invention is to overcome the defects of the prior art and provide a cold heading steel treatment method without adding aluminum slag.

[0006] The technical problem solved by this invention is achieved by the following technical solution.

[0007] This invention provides a method for treating cold-headed steel without adding aluminum slag, comprising the following steps:

[0008] When tapping steel from the converter, high manganese and aluminum-iron are first added for alloying, and then lime is added for slag washing.

[0009] The molten steel is sampled at the argon station, and the amount of aluminum wire fed in is increased according to the acid-soluble aluminum content in the molten steel.

[0010] After the molten steel is fed into the LF furnace, lime, fluorite, and synthetic slag are added. Argon gas is passed through and stirred under power supply. The argon gas is then reduced, and a first sample is taken. The color of the slag is observed. After the first sample is taken, aluminum wire is fed and lime is added according to the acid-soluble aluminum content of the molten steel and the color of the refining slag. Argon gas is passed through and stirred. A second sample is taken. The acid-soluble aluminum content of the molten steel is controlled to be 0.030%-0.035%, the silicon content to be 0.03%-0.06%, and the sulfur content to be <0.007%. Calcium wire is fed and soft blowing is performed to complete the LF furnace refining process.

[0011] The present invention has the following beneficial effects:

[0012] The present invention provides a method for cold heading steel treatment without adding aluminum slag. The method does not use aluminum slag in the entire smelting process, which greatly reduces the generation of flue gas, avoids dust, and ensures the quality of molten steel. Detailed Implementation

[0013] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0014] The following is a detailed description of a cold heading steel treatment method without adding aluminum slag provided by an embodiment of the present invention.

[0015] This invention provides a method for treating cold-heading steel without adding aluminum slag, comprising the following steps:

[0016] 1. During converter tapping, argon gas at a flow rate of 40 cubic meters per hour is used. When the steel is tapped to 1 / 3 capacity, 1050 kg of high-manganese per 120 tons of molten steel and 350 kg of ferroaluminum per 120 tons of molten steel are added. When the steel is tapped to 3 / 4 capacity, 500 kg of lime per 120 tons of molten steel is added. By changing the order of slag addition—alloying first followed by slag washing—the high aluminum content in the molten steel will combine with oxygen to form aluminum oxide, which easily forms large, coral-like inclusions that float quickly. Adding slag later in the tapping process can adsorb these inclusions. Compared to the original method, the purity of the molten steel is higher because the original technique involved slag washing followed by alloying. The oxygen in the molten steel would oxidize the slag, generating other oxides. After the ferroaluminum was added, it could not reduce the oxides in the slag, and these oxides would then further oxidize the molten steel.

[0017] 2. Because the aluminum-iron is added earlier, the acid-soluble aluminum content in the molten steel is lower compared to the original technology (the earlier it is added, the longer the oxidation time, and naturally the lower the content). Therefore, more aluminum wire will be fed into the argon station. Compared to the original technology, an average of 36.3 meters more aluminum wire is fed per furnace.

[0018] 3. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Power on for 500-700 seconds, then stir with argon gas at 100 m³ / h for 100-150 seconds. Reduce the argon gas flow to 10-20 m³ / h, take a sample, observe the slag, and check the slag color (white, green, black). Once the sample is ready, add aluminum slag and feed aluminum wire according to the acid-soluble aluminum composition and slag color. For white slag, adjust the acid-soluble aluminum to 0.050%- For green slag, add 170-200 kg of lime per 120 tons of molten steel to adjust the acid-soluble aluminum content to 0.06-0.065%. For black slag, add 230-260 kg of lime per 120 tons of molten steel to adjust the acid-soluble aluminum content to 0.075%-0.080%. Stir with 100 cubic meters per hour of argon gas for 4, 5, and 6 minutes respectively. Take sample two and adjust the content to 0.030%-0.035% based on the acid-soluble aluminum content. If the acid-soluble aluminum content of sample two is 0.035%-0.048%, then no additional aluminum wire is needed.

[0019] After power is supplied to the station, stirring is required, mainly for pre-desulfurization to control the sulfur content below 0.007%. Lower sulfur levels indicate better slag, which allows for longer and greater adsorption of inclusions from the molten steel. In practice, situations may arise where sulfur cannot be effectively removed, such as when the converter steel has high oxygen content, slag is discharged during tapping, or the amount of deoxidized alumina added is insufficient. In these cases, the slag will not be white when taking the first sample from the refining process, requiring abnormal handling. For green slag, add 170-200 kg of lime per 120 tons of molten steel, adjusting the acid-soluble alumina content to 0.06-0.065%. For black slag, add 230-260 kg of lime per 120 tons of molten steel, adjusting the acid-soluble alumina content to 0.075%-0.080%, stirring for 5-6 minutes respectively.

[0020] Once the sample is ready, the acid-soluble aluminum and lime should be prepared according to the composition and slag color, and the stirring time should be controlled. The main purpose is to enhance the reducing properties of the slag, which we judge using the reduction of silicon. According to the oxidation order of elements, the order is: potassium, calcium, sodium, magnesium, aluminum, silicon, manganese... Since the main elements of this steel grade are calcium, aluminum, silicon, and manganese, and calcium is fed last, we look at the silicon element. If silicon can be reduced, it means that the weaker oxidizing elements such as iron and manganese in the slag can also be reduced. Therefore, after the first sample is produced, aluminum slag is added and aluminum feed wire is fed according to the composition of acid-soluble aluminum and the color of slag. For white slag, the acid-soluble aluminum is prepared to 0.050%-0.055%. For green slag, 170-200 kg of lime / 120 tons of molten steel is added, and the acid-soluble aluminum is prepared to 0.06-0.065%. For black slag, 230-260 kg of lime / 120 tons of molten steel is added, and the acid-soluble aluminum is prepared to 0.075%-0.080%. Argon gas at 100 cubic meters / hour is used to stir for 4, 5 and 6 minutes respectively. In practice, without slag discharge and without residual silicon in the ladle, silicon reduction of 0.002%-0.004% can be achieved by controlling the range of acid-soluble aluminum and the amount of lime added, thus controlling the silicon content in the molten steel to 0.03-0.06%. If it is found that the silicon in the molten steel has not been reduced when sampling the second sample after stirring, it indicates that the slag's reduction capacity is still insufficient. In this case, it is necessary to continue adding 130-200 kg of lime per 120 tons of molten steel, while manually adding 20-40 kg of aluminum granules per 120 tons of molten steel. Based on the acid-soluble aluminum content of the first sample, prepare the solution to 0.050%, stir with 100 cubic meters per hour of argon for 2-3 minutes, and then take the third sample. Only when it is confirmed that silicon can be reduced and the silicon content in the molten steel is greater than 0.03% can calcium wire be fed for soft blowing.

[0021] By following the above steps, aluminum dross can be avoided, dust can be prevented, and the quality of molten steel can be guaranteed.

[0022] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0023] Example 1

[0024] A method for treating cold-heading steel without adding aluminum slag

[0025] 1. When tapping steel from the converter, use argon gas at a flow rate of 40 cubic meters per hour. When the steel is tapped to 1 / 3 full, add 1050 kg of high manganese per 120 tons of molten steel and 350 kg of aluminum ferroalloy per 120 tons of molten steel. When the steel is tapped to 3 / 4 full, add 500 kg of lime per 120 tons of molten steel.

[0026] 2. When the molten steel arrives at the argon station, a sample is taken. After the sample is tested, the aluminum content is 0.031%. Calculate by increasing the aluminum content by 0.001% for every 5 meters, and feed an additional 130 meters of aluminum wire to increase the aluminum content to 0.057%, controlling it between 0.040% and 0.060%.

[0027] 3. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Use argon gas at a flow rate of 55 cubic meters per hour. Power the electrodes with an active power of 12500 kW for 700 seconds, then stir with argon gas at a flow rate of 100 cubic meters per hour for 130 seconds. Reduce the argon gas flow rate to 10 cubic meters per hour. Take one sample, observe the slag, and check its color (white, no slag adjustment needed). After sample one is obtained, the molten steel should contain 0.022% silicon, 0.006% sulfur, and acid... Aluminum content is 0.048%. 35 meters of aluminum wire are fed according to the acid-soluble aluminum composition. White slag is produced. The acid-soluble aluminum content is adjusted to 0.055%. The mixture is stirred with 100 cubic meters per hour of argon gas for 4 minutes. Two samples are taken. After analysis, the sulfur content of the molten steel is 0.004%, silicon 0.042%, and acid-soluble aluminum 0.036% (aluminum wire is not needed if the content is between 0.035% and 0.045%). The temperature is then measured and raised to the outlet temperature +15°C. 160 meters of calcium wire / 120 tons of molten steel are fed in, and the mixture is gently blown out with 7 cubic meters per hour of argon gas for 15 minutes before exiting the station.

[0028] Example 2

[0029] A method for treating cold-heading steel without adding aluminum slag

[0030] 1. When tapping steel from the converter, use argon gas at a flow rate of 40 cubic meters per hour. When the steel is tapped to 1 / 3 full, add 1050 kg of high manganese per 120 tons of molten steel and 350 kg of aluminum ferroalloy per 120 tons of molten steel. When the steel is tapped to 3 / 4 full, add 500 kg of lime per 120 tons of molten steel.

[0031] 2. When the molten steel arrives at the argon station, a sample is taken. After the sample is tested, the aluminum content is 0.018%. 150 meters of aluminum wire is fed in, and the aluminum content is adjusted to 0.048%. The argon gas is then turned off and the molten steel is transferred to the LF furnace.

[0032] 3. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Use argon gas at a flow rate of 45 cubic meters per hour, with the electrode active power at 12500 kW for 500 seconds. Then, cut off the power and stir with argon gas at a flow rate of 100 cubic meters per hour for 140 seconds. Reduce the argon gas flow rate to 10 cubic meters per hour, take a sample, observe the slag, and check the slag color (green slag, requiring slag material adjustment). After the first sample is obtained, the molten steel should contain 0.015% silicon, 0.009% sulfur, and 0.037% acid-soluble aluminum. Based on the acid-soluble aluminum composition and slag color, add aluminum slag and feed the slag. For aluminum wire, add 185 kg of lime to 120 tons of molten steel and feed 130 meters of aluminum wire. The acid-soluble aluminum content is adjusted to 0.063%. Stir with 100 cubic meters / hour of argon gas for 5 minutes. Take two samples. Sample two contains 0.036% silicon, 0.006% sulfur, and 0.026% acid-soluble aluminum. Based on the acid-soluble aluminum content, add another 40 meters of aluminum wire to 120 tons of molten steel, adjusting the content to 0.034%. After feeding the aluminum wire, wait for 5 minutes with 15 cubic meters / hour of argon gas, then measure the temperature and raise it to the outlet temperature +15℃. Feed 190 meters of calcium wire to 120 tons of molten steel, and gently blow with 8 cubic meters / hour of argon gas for 17 minutes before exiting the station.

[0033] Example 3

[0034] A method for treating cold-heading steel without adding aluminum slag

[0035] 1. When tapping steel from the converter, use argon gas at a flow rate of 40 cubic meters per hour. When the steel is tapped to 1 / 3 full, add 1050 kg of high manganese per 120 tons of molten steel and 350 kg of aluminum ferroalloy per 120 tons of molten steel. When the steel is tapped to 3 / 4 full, add 500 kg of lime per 120 tons of molten steel.

[0036] 2. When molten steel arrives at the argon station, an average of 36.3 meters of aluminum wire is fed per furnace.

[0037] 3. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Use argon gas at a flow rate of 50 m³ / h. Power is supplied to the electrodes at a power output of 12500 kW for 650 seconds. Power is then cut off, and the mixture is stirred with argon gas at a flow rate of 100 m³ / h for 125 seconds. The flow rate is then reduced to 15 m³ / h. Take one sample, observe the slag adhesion and color (black slag). After sample one is obtained, the molten steel should contain 0.016% silicon, 0.012% sulfur, and 0.018% acid-soluble aluminum. Based on the acid-soluble aluminum composition and slag color, add aluminum slag and feed aluminum wire. For the black slag, add 260 kg of lime / 120 tons of molten steel and 300 meters of aluminum wire / 120 tons of molten steel. Acid-soluble aluminum... The solution was prepared to 0.078%, and stirred with argon gas at a rate of 100 cubic meters per hour for 6 minutes. Sample 2 was taken, which contained 0.007% sulfur, 0.025% silicon, and 0.032% acid-soluble aluminum. Since the silicon content in the molten steel was less than 0.03%, it indicated that the slag's reducing capacity was still insufficient. Therefore, 150 kg of lime per 120 tons of molten steel needed to be added, along with 20 kg of aluminum granules by hand. Based on the acid-soluble aluminum content of Sample 2, 90 meters of aluminum wire per 120 tons of molten steel was fed in, and the acid-soluble aluminum content was prepared to 0.050%. The solution was stirred with argon gas at a rate of 100 cubic meters per hour for 3 minutes. Sample 3 was then taken, which contained 0.037% silicon, 0.005% sulfur, and 0.037% acid-soluble aluminum in the molten steel. Only when it was confirmed that silicon could be reduced and the silicon content in the molten steel was greater than 0.03% could calcium wire be fed for soft blowing. Raise the temperature to the exit temperature +15℃, feed in 200 meters of calcium wire / 120 tons of molten steel, and use 8 cubic meters / hour of argon gas for a soft blowing process for 19 minutes before exiting the station.

[0038] Comparative Example 1

[0039] 1. When tapping steel from the converter, use 40 cubic meters / hour of argon gas. When the steel is tapped to 1 / 3, add 500 kg of lime per 120 tons of molten steel. When the steel is tapped to 3 / 4, add 1050 kg of high manganese per 120 tons of molten steel and 350 kg of aluminum ferroalloy per 120 tons of molten steel.

[0040] 2. When the molten steel arrives at the argon station, a sample is taken. After the sample is tested, the aluminum content is 0.031%, and the steel is discharged directly from the station.

[0041] 3. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Use argon gas at a flow rate of 55 cubic meters per hour. The electrode active power is 12500 kW, and the power is supplied for 300 seconds. Then reduce the argon gas flow rate to 10 cubic meters per hour. Take one sample, observe the slag, and check its color (green). After sample one is obtained, the molten steel should contain 0.012% silicon, 0.009% sulfur, and 0.012% acid-soluble aluminum. Feed the appropriate amount of acid-soluble aluminum according to the aluminum composition. 150 meters of aluminum wire per 120 tons of molten steel, acid-soluble aluminum is prepared to 0.042%, stirred with 100 cubic meters / hour of argon gas for 4 minutes, and two samples are taken. After analysis, the sulfur content of the molten steel is 0.010%, silicon 0.021%, and acid-soluble aluminum 0.025%. Then feed another 50 meters of aluminum wire per 120 tons of molten steel, prepared to 0.035%, and measure the temperature again. Raise the temperature to the outlet temperature +15℃, and feed in 160 meters of calcium wire per 120 tons of molten steel. Use 7 cubic meters / hour of argon gas for soft blowing for 15 minutes before leaving the station.

[0042] Comparative Example 2

[0043] Similar to the steps in Example 1, the only difference is that the order of adding the slag and the alloy is changed.

[0044] Adding slag first can pre-decompose the slag and remove some of the oxygen. Then adding realloy can improve the alloy yield. However, since this steel is aluminum-containing steel, the aluminum oxide particles that are oxidized by the deoxidized slag will become smaller particles, which is not conducive to the removal of aluminum oxide.

[0045] Comparative Example 3

[0046] The steps are similar to those in Example 1, except that after sampling at the argon station, the acid-soluble aluminum is not controlled within the range of 0.04-0.06.

[0047] If the concentration is below the range, such as 0.025%, the acid-soluble aluminum content will be low when the molten steel arrives at the LF furnace. This will reduce the chance of white slag at the first sampling point and increase the chance of green or black slag. Therefore, the probability of adjusting the slag material after the first sampling point or even after the second sampling point is high. Relatively speaking, the later the slag is prepared, the worse it is for the quality of the molten steel.

[0048] However, if too much aluminum wire is fed into the argon station, exceeding the upper limit, for example, as high as 0.080%, then the slag in the molten steel after reaching the LF furnace will have low oxygen content and poor slag fluidity. During refining and slag formation, a relatively large amount of fluorite will be added to adjust the slag. On the other hand, if a large amount of aluminum wire is fed into the argon station, resulting in a surplus of acid-soluble aluminum in the molten steel, there will still be a surplus after refining and slag formation. If the acid-soluble aluminum content in the molten steel is higher than 0.045%, then the refining process will resort to methods such as limiting the blowing of slag to reduce acid-soluble aluminum, or using more fluorite to dilute the slag to reduce acid-soluble aluminum, which is also bad for the quality of the molten steel.

[0049] In summary, the argon station uses acid to dissolve aluminum based on the composition of samples taken after steel tapping, which is a step in the process control of deoxidation, desulfurization, slag formation, and acid-dissolving aluminum in the LF furnace.

[0050] Comparative Example 4

[0051] Similar to the steps in Example 1, the only difference is that the slag-forming time before sampling is less than 500 seconds, for example, 300 seconds. This would create the illusion that the acid-dissolved aluminum in the molten steel is too high, even though it is not actually high. This is because a certain amount of time is needed during the slag-forming process for the acid-dissolved aluminum in the molten steel to react with the slag. If the reaction is incomplete, that is, if the slag-forming time is insufficient, only part of the oxygen in the slag will be removed, and some oxygen will continue to be removed after sampling, resulting in a large consumption of acid-dissolved aluminum in the molten steel. This is not conducive to the precise control of acid-dissolved aluminum.

[0052] Comparative Example 5

[0053] Similar to the steps in Example 1, the only difference is that no stirring is performed before sampling one; sampling is done immediately after power supply is completed. In this case, the sulfur content in the first sample will be relatively high, making it difficult to reduce it below 0.007%. Sulfur in molten steel affects the yield of calcium feed wire in the later stages of refining; the lower the sulfur content, the higher the calcium yield. Furthermore, if no stirring is performed before sampling one, the reaction between the slag and molten steel may not be sufficient, and the amount of slag adhering to the slag may not be accurate, which will also affect subsequent slag conditioning and the quality of the molten steel.

[0054] Comparative Example 6

[0055] Similar to the steps in Example 1, the only difference is that when taking the sample, lime and aluminum feed are not added according to the color of the slag. For example, in the green slag in Comparative Example 1, the acid-dissolved aluminum is 0.012%, the aluminum feed wire is 150 meters long, the acid-dissolved aluminum is adjusted to 0.042%, and it is stirred with argon gas at 100 cubic meters / hour for 4 minutes.

[0056] Because the slag was not whitened, no lime was added, and the aluminum wire deoxidation was insufficient, the slag did not improve when the second sample was taken. In fact, it deteriorated into glass slag, which greatly reduced its ability to adsorb inclusions. Thus, even if all the components were qualified in the end, the inclusions in the molten steel would still be relatively high.

[0057] Therefore, it is necessary to observe the slag and adjust it, making the slag white as early as possible, or even immediately after sample one, to avoid adjustments after sample two. Example 3 is an abnormal handling procedure. The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for treating cold-heading steel without adding aluminum slag, characterized in that, Includes the following steps: When tapping steel from the converter, high manganese and aluminum-iron are first added for alloying, and then lime is added for slag washing. The molten steel is sampled at the argon station, and the amount of aluminum wire fed in is increased according to the acid-soluble aluminum content in the molten steel. After the molten steel is fed into the LF furnace, lime, fluorite, and synthetic slag are added. Argon gas is passed through and stirred under power supply. The argon gas is then reduced, and a first sample is taken. The color of the slag is observed. After the first sample is taken, aluminum wire is fed and lime is added according to the acid-soluble aluminum content of the molten steel and the color of the refining slag. Argon gas is passed through and stirred. A second sample is taken. The acid-soluble aluminum content of the molten steel is controlled to be 0.030%-0.035%, the silicon content to be 0.03%-0.06%, and the sulfur content to be <0.007%. Calcium wire is fed and soft blowing is performed to complete the LF furnace refining process. The feeding of aluminum wire and the addition of lime are based on the composition of acid-soluble aluminum in molten steel and the color of refining slag. If the refining slag is white slag, feed aluminum wire into the molten steel to adjust the acid-soluble aluminum content to 0.050%-0.055%, and stir with argon gas at 100 cubic meters / hour for 4 minutes. The feeding of aluminum wire and the addition of lime are based on the composition of acid-soluble aluminum in molten steel and the color of refining slag. If the refining slag is green slag, feed aluminum wire into the molten steel to adjust the acid-soluble aluminum content to 0.06-0.065%, and add 170-200 kg of lime per 120 tons of molten steel. Stir with 100 cubic meters per hour of argon gas for 5 minutes. The feeding of aluminum wire and the addition of lime are based on the composition of acid-soluble aluminum in molten steel and the color of refining slag. If the refining slag is black slag, aluminum wire is fed into the molten steel to adjust the acid-soluble aluminum content to 0.075%-0.080%, and 230-260 kg of lime / 120 tons of molten steel is added. The mixture is stirred for 6 minutes with 100 cubic meters / hour of argon gas. It also includes: after the steel is tapped from the converter, a sample is taken at the argon station. Then, based on the acid-soluble aluminum content in the steel sample, if it is less than 0.040%, aluminum wire is added, calculated at 0.001% acid-soluble aluminum per 5 meters, to reach 0.040%-0.060%. If it is greater than 0.060%, aluminum wire is not needed, the argon gas is turned off directly, and the molten steel is transferred to the LF furnace. After the molten steel is added to the LF furnace, add 350 kg of lime / 120 tons of molten steel, 60 kg of fluorite / 120 tons of molten steel, and 500 kg of synthetic slag / 120 tons of molten steel. Power is supplied for 500-700 seconds, and argon gas is stirred at 100 cubic meters / hour for 100-150 seconds. The argon gas flow rate is then reduced to 10-20 cubic meters / hour, and one sample is taken.

2. The cold heading steel treatment method according to claim 1, characterized in that, When tapping steel from the converter, argon gas at a flow rate of 40 cubic meters per hour is used. When the steel is tapped to 1 / 3 of its capacity, 1050 kg of high manganese per 120 tons of molten steel and 350 kg of aluminum ferroalloy per 120 tons of molten steel are added. When the steel is tapped to 3 / 4 of its capacity, 500 kg of lime per 120 tons of molten steel is added.

3. The cold heading steel treatment method according to claim 1, characterized in that, The refining process is energized continuously from the start of power supply to the exit of the station, with an active power of 9000-12500kW.

4. The cold heading steel treatment method according to claim 1, characterized in that, For sample two, based on the acid-soluble aluminum composition of the molten steel, the acid-soluble aluminum content is adjusted to 0.030%-0.035%. If the acid-soluble aluminum content in sample two is 0.035%-0.048%, no additional aluminum wire is required.

5. The cold heading steel treatment method according to claim 1, characterized in that, If the silicon content in the molten steel is less than 0.03% when taking sample two, it is necessary to continue adding 130-200 kg of lime per 120 tons of molten steel, and at the same time manually add 20-40 kg of aluminum granules per 120 tons of molten steel. Based on the acid-soluble aluminum content of sample two, adjust the acid-soluble aluminum content to 0.050%, stir with argon gas at 100 cubic meters per hour for 2-3 minutes, and then take sample three to confirm that silicon can be reduced. When the silicon content in the molten steel is greater than 0.03%, then feed calcium wire for soft blowing.

Citation Information

Patent Citations

  • Low-carbon aluminum-containing cold forging steel smelting process

    CN114836593A

  • LF refining method of CH1T ultra-low carbon cold forging steel

    CN115261560A