Stem cell climbing degradable scaffold and preparation method and application thereof
By using degradable collagen-gelatin mixed gelatin and coupled natural protein modification on cell culture scaffolds, simulated extracellular matrix is constructed, and the problems of insufficient biological activity and difficulty in degradation are solved, and directed differentiation of stem cells and in vivo tissue repair are achieved.
Patent Information
- Application Number
- CN202311777350.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The existing cell culture scaffolds have insufficient biological activity and are not easy to degrade and absorb, which limits the application of tissue engineering components.
Degradable collagen-gelatin mixed gelatin is used as the scaffolding framework, and active groups are introduced through air plasma treatment and coupled natural proteins and growth factors are modified on their surface to construct a microenvironment that simulates the extracellular matrix.
The bioactive stability and degradability of the scaffold are achieved, supporting cell adhesion, proliferation and directed differentiation, and are suitable for in vivo tissue repair.
Smart Images

Figure CN117752859B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tissue engineering, and in particular to a stem cell climbing degradable scaffold and a preparation method and application thereof. Background Art
[0002] Currently, in the field of tissue engineering, using stem cells to construct tissue engineering components to achieve organ and tissue regeneration and repair is a hot topic and difficulty in research. However, most of the cell culture scaffolds commonly used in tissue engineering are made of non-degradable materials, and the existing extracellular matrix simulation materials are insufficiently bioactive and lack biological activity, which is not conducive to cell adhesion and directional differentiation, which limits the application of the constructed tissue engineering components. In addition, there are also methods that use layer-by-layer self-assembly technology to modify biological molecules on the surface of the scaffold, but the preparation process is relatively complicated and the bioactive modification is unstable.
[0003] Therefore, developing a new stem cell culture scaffold that simulates the bioactive interface of the natural extracellular matrix and has degradability so that it can serve as an extracellular matrix that can both support cell growth and be degraded and absorbed after implantation in the body is a technical challenge in the current field of tissue engineering. Summary of the invention
[0004] In order to solve the problems of insufficient biological activity, difficulty in degradation and absorption, and limited application of existing cell culture scaffolds, the present invention provides a stem cell climbing degradable scaffold and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0006] The method for preparing the stem cell-climbing degradable scaffold of the present invention mainly comprises the following steps:
[0007] 1) Take collagen powder and gelatin powder, add buffer solution, stir until dissolved, and prepare collagen-gelatin mixed glue;
[0008] 2) treating a medical-grade porous polylactic acid scaffold with air plasma to introduce active groups;
[0009] 3) pouring the collagen-gelatin mixed glue obtained in step 1) into the treated medical-grade porous polylactic acid scaffold, and preparing the scaffold after freeze-drying;
[0010] 4) dissolving laminin in PBS buffer and soaking the scaffold prepared in step 3) to perform coupling reaction to obtain a mixed solution;
[0011] 5) Add growth factors to the mixed solution and continue to soak the scaffold to finally obtain a biodegradable scaffold with stem cells climbing on it.
[0012] As a preferred embodiment, the mass ratio of the collagen powder to the gelatin powder is (1:5) to (5:1), and the concentration range of the mixture of the collagen powder and the gelatin powder is 0.1% to 1%.
[0013] As a preferred embodiment, the buffer solution is an acetate buffer solution with a concentration of 0.01M to 1M, a pH of 2 to 5, and a temperature of 0°C to 60°C.
[0014] As a preferred embodiment, in the collagen-gelatin mixed gel, the total mass fraction of the collagen powder and the gelatin powder is 0.1% to 10%.
[0015] As a preferred embodiment, the pore size of the medical-grade porous polylactic acid scaffold is 90 μm to 110 μm.
[0016] As a preferred embodiment, laminin is dissolved in PBS buffer to obtain a mixture, wherein the mass fraction of laminin in the mixture is 0.1% to 10%.
[0017] As a preferred embodiment, in step 4), the scaffold prepared in step 3) is immersed for 3-5 hours to carry out coupling reaction; in step 5), the scaffold is further immersed for 10-14 hours to obtain a stem cell-climbing degradable scaffold.
[0018] As a preferred embodiment, the growth factors are bFGF and EGF, the amount of bFGF added is 10 ng / ml to 10 μg / ml, and the amount of EGF added is 1 ng / ml to 10 μg / ml.
[0019] The invention provides a method for preparing a stem cell-climbing degradable scaffold, and a stem cell-climbing degradable scaffold prepared by the method.
[0020] The invention provides an application of the stem cell-climbing degradable scaffold in the preparation of in vivo tissue repair medicine.
[0021] The beneficial effects of the present invention are:
[0022] The purpose of the present invention is to provide a novel stem cell-climbing degradable scaffold by constructing a bioactive scaffold surface that simulates the natural extracellular matrix, as well as a preparation method and application of the scaffold. Compared with the prior art, the present invention has the following advantages:
[0023] (1) The present invention uses a degradable collagen-gelatin mixture as the stent skeleton. The collagen-gelatin mixture can be degraded and absorbed in the body without causing a foreign body reaction, thus avoiding the problem that a traditional stent requires a second removal surgery.
[0024] (2) The stem cell climbing biodegradable scaffold prepared by the present invention uses air plasma treatment to directly introduce active groups into the scaffold, and then directly couples natural proteins. Directly coupling natural biomacromolecules without surface modification avoids the complex process of layer-by-layer modification and ensures the stability of the biological activity of the interface. The directly coupled biomacromolecules maintain their natural structure and have strong biological activity.
[0025] (3) The stem cell-climbing degradable scaffold prepared by the present invention, by coupling natural matrix molecules such as laminin, constructs a microenvironment simulating the extracellular matrix on the scaffold surface, which is conducive to cell adhesion and function. Further addition of growth factors can stimulate the directional differentiation of target cells.
[0026] (4) By culturing stem cells on the prepared stem cell-climbing biodegradable scaffold, the stem cells can adhere to the scaffold surface and grow and differentiate in a directed manner to form tissue engineering building blocks that can be implanted in the body, thereby achieving tissue repair. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a process flow chart of the preparation method of the stem cell climbing degradable scaffold of the present invention.
[0028] Figure 2 This is a cross-sectional structural diagram of the stem cell-climbing degradable scaffold prepared in the present invention.
[0029] Figure 3 The figure is a growth diagram of bone marrow mesenchymal stem cells on the stem cell climbing layer degradable scaffold prepared by the present invention. DETAILED DESCRIPTION
[0030] The stem cell climbing degradable scaffold and its preparation method of the present invention solve the problems of insufficient biological activity, difficulty in degradation and absorption, and limited application of existing cell culture scaffolds. The present invention achieves the function of simulating natural extracellular matrix to guide the directional differentiation of stem cells, and the function of degradation and absorption after implantation in the body.
[0031] like Figure 1 As shown, the preparation method of the stem cell climbing degradable scaffold of the present invention mainly comprises the following steps:
[0032] 1) Take collagen powder and gelatin powder, add buffer solution, stir until dissolved, and prepare collagen-gelatin mixed glue;
[0033] 2) treating a medical-grade porous polylactic acid scaffold with air plasma to introduce active groups;
[0034] 3) pouring the collagen-gelatin mixed glue obtained in step 1) into the treated medical-grade porous polylactic acid scaffold, and preparing the scaffold after freeze-drying;
[0035] 4) dissolving laminin in PBS buffer and soaking the scaffold prepared in step 3) to perform coupling reaction to obtain a mixed solution;
[0036] 5) Add growth factors to the mixed solution and continue to soak the scaffold to finally obtain a biodegradable scaffold with stem cells climbing on it.
[0037] The stem cell-climbing degradable scaffold prepared by the method for preparing the stem cell-climbing degradable scaffold of the present invention can be used to prepare in vivo tissue repair drugs.
[0038] The stem cell climbing layer degradable scaffold prepared by the present invention has good cell compatibility, is conducive to the directional differentiation of cells, and can be degraded and absorbed after being implanted in the body.
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] Example 1 Preparation of Stem Cell Climbing Degradable Scaffold
[0041] 1) Take 0.5 g collagen powder and 0.5 g gelatin powder, add 100 ml of 0.05 M acetate buffer solution with a pH of 3, stir to dissolve, and prepare a 1% collagen-gelatin mixed gel;
[0042] 2) taking a medical-grade porous polylactic acid scaffold (pore size 100 μm) and subjecting it to air plasma treatment to introduce carboxyl groups;
[0043] 3) pouring the solution prepared by collagen-gelatin mixed gel into the treated polylactic acid scaffold, and freeze-drying to obtain the scaffold;
[0044] 4) 5 mg of laminin was dissolved in 100 ml of PBS buffer and the scaffold prepared in step 3) was immersed in the scaffold for 4 hours for coupling;
[0045] 5) Add 10 ng / ml of growth factors bFGF and EGF to the mixed solution, and continue to soak the stem cells in the biodegradable scaffold for 12 hours.
[0046] Example 2 Preparation of Stem Cell Climbing Degradable Scaffold
[0047] 1) Take 0.5 g collagen powder and 1.5 g gelatin powder, add 100 ml of 0.08 M acetate buffer solution with a pH of 4, stir to dissolve, and prepare a 5% collagen-gelatin mixed gel;
[0048] 2) taking a medical-grade porous polylactic acid scaffold (pore size 100 μm) and subjecting it to air plasma treatment to introduce carboxyl groups;
[0049] 3) pouring the solution prepared by collagen-gelatin mixed gel into the treated polylactic acid scaffold, and freeze-drying to obtain the scaffold;
[0050] 4) 5 mg of laminin was dissolved in 100 ml of PBS buffer and the scaffold prepared in step 3) was immersed in the scaffold for 3 hours for coupling;
[0051] 5) Add 20 ng / ml of growth factors bFGF and EGF to the mixed solution, and continue to soak the stem cells in the biodegradable scaffold for 10 hours.
[0052] Example 3 Preparation of Stem Cell Climbing Degradable Scaffold
[0053] 1) Take 1.5 g collagen powder and 0.5 g gelatin powder, add 100 ml of 0.05 M acetate buffer solution with a pH of 5, stir to dissolve, and prepare a 7% collagen-gelatin mixed gel;
[0054] 2) taking a medical-grade porous polylactic acid scaffold (pore size 100 μm) and subjecting it to air plasma treatment to introduce carboxyl groups;
[0055] 3) pouring the solution prepared by collagen-gelatin mixed gel into the treated polylactic acid scaffold, and freeze-drying to obtain the scaffold;
[0056] 4) 5 mg of laminin was dissolved in 100 ml of PBS buffer and the scaffold prepared in step 3) was immersed in the scaffold for 5 hours for coupling;
[0057] 5) Add 30 ng / ml of growth factors bFGF and EGF to the mixed solution, and continue to soak the stem cells in the biodegradable scaffold for 14 hours.
[0058] Experimental Example 1 Directed differentiation of bone marrow mesenchymal stem cells on a stem cell-climbing biodegradable scaffold
[0059] 1) Bone marrow mesenchymal stem cells were inoculated on the stem cell-climbing biodegradable scaffold prepared in Example 1 at a density of 10,000 cells / cm 2 ;
[0060] 2) The culture medium was low-glucose DMEM medium containing 10% fetal bovine serum, and the culture medium was replaced every 2 days;
[0061] 3) The incubator conditions were 37°C, 5% CO2, and saturated humidity for 7 days;
[0062] 4) Using cell activity plant enzymes and calcification nodule staining, the growth and calcification of bone marrow mesenchymal stem cells on the stem cell climbing biodegradable scaffold after 7 days of culture were observed.
[0063] The stem cell climbing layer degradable scaffold prepared by the present invention is biodegradable, and the surface is modified by direct coupling with natural biomacromolecules to construct a bioactive interface that simulates the extracellular matrix, which can effectively support the adhesion, proliferation and directional differentiation of stem cells. On this basis, stem cells are cultured to obtain tissue engineering building blocks, and after implanting them into the body, the stem cells rely on the stem cell climbing layer degradable scaffold to absorb blood nutrients, proliferate around the lesion and transform into vascular endothelial cells, which is beneficial to the repair of the vascular wall. When the scaffold is degraded, the vascular wall is restored to a normal state, and the tissue repair effect is played before being degraded and absorbed.
[0064] The present invention discloses a stem cell climbing degradable scaffold and its preparation method and application. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar replacements and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The product of the present invention has been described through a preferred embodiment, and relevant personnel can obviously modify or appropriately change and combine the products described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
Claims
1. A method for preparing a stem cell-climbing degradable scaffold, characterized in that: The following steps are involved: 1) taking collagen powder and gelatin powder, adding buffer solution, stirring until dissolved, and preparing collagen-gelatin mixed glue; the mass ratio of the collagen powder to the gelatin powder is (1:5) to (5:1), and the concentration range of the mixture of the collagen powder and the gelatin powder is 0.1% to 1%; The buffer solution is an acetate buffer solution with a concentration of 0.01M to 1M, a pH of 2 to 5, and a temperature of 0°C to 60°C; In the collagen-gelatin mixed gel, the total mass fraction of the collagen powder and gelatin powder is 0.1% to 10%; 2) treating a medical-grade porous polylactic acid scaffold with air plasma to introduce active groups; the pore size of the medical-grade porous polylactic acid scaffold is 90 μm to 110 μm; 3) pouring the collagen-gelatin mixed glue obtained in step 1) into the treated medical-grade porous polylactic acid scaffold, and preparing the scaffold after freeze-drying; 4) dissolving laminin in PBS buffer and soaking the scaffold obtained in step 3) for 3-5 hours to perform coupling reaction to obtain a mixed solution; the mass fraction of laminin in the mixed solution is 0.1% to 10%; 5) Adding growth factors to the mixed solution, continuing to soak the scaffold for 10-14 hours, and finally obtaining a stem cell climbing degradable scaffold; the growth factors are bFGF and EGF, the amount of bFGF added is 10ng / ml to 10μg / ml, and the amount of EGF added is 1ng / ml to 10μg / ml.
2. The stem cell-climbing degradable scaffold prepared by the preparation method of the stem cell-climbing degradable scaffold as described in claim 1.
3. Use of the stem cell-climbing degradable scaffold as claimed in claim 2 in the preparation of in vivo tissue repair drugs.