Titanium-doped anhydrous iron phosphate material and preparation method and application thereof

By controlling the mixing ratio of titanium ferrous sulfate and titanium-free ferrous sulfate and the oxidation reaction, a stable titanium-containing anhydrous iron phosphate material was prepared, solving the problem of unstable titanium content and improving the performance of battery materials and waste utilization efficiency.

CN117756076BActive Publication Date: 2024-11-12HUBEI HONGRUN HIGH-TECH NEW MATERIALS CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311785880.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-12
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

In existing technologies, the content of titanium doping in anhydrous iron phosphate is unstable, resulting in uneven performance of lithium iron phosphate batteries. Furthermore, traditional titanium doping methods require additional materials or have high energy consumption, making it difficult to achieve stable control.

Method used

A slurry containing ferrous sulfate containing titanium and ferrous sulfate without titanium was prepared by mixing the raw material solutions and controlling the ratio and reaction of the oxidant. The slurry was then aged, rinsed, dried and sintered to form titanium-doped anhydrous ferric phosphate material. The titanium element in the by-products of titanium dioxide was used as the dopant source to achieve stable control of the titanium element.

Benefits of technology

Anhydrous iron phosphate material with stable titanium content was prepared, exhibiting a uniform nanoscale particle stacking morphology, which improves the performance and product quality of battery materials, and realizes waste utilization and low-energy production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117756076B_ABST
    Figure CN117756076B_ABST
Patent Text Reader

Abstract

The present invention provides a titanium-doped anhydrous iron phosphate material and a preparation method and application thereof, belonging to the technical field of iron phosphate material preparation. The preparation method of the titanium-doped anhydrous iron phosphate material comprises the steps of: providing a titanium-containing ferrous sulfate raw material liquid and a titanium-free ferrous sulfate raw material liquid; mixing the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid to obtain a mixed solution; mixing the mixed solution with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate; aging, rinsing, drying and sintering the slurry in sequence to obtain the titanium-doped anhydrous iron phosphate material. The present invention can achieve doping control of the titanium element in the titanium-doped anhydrous iron phosphate material by adjusting the mixing ratio of the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid, so that the titanium element content in the final product is stable and controllable; the titanium-doped anhydrous iron phosphate material has a uniform nano-scale particle stacking morphology, which is conducive to the application of preparing battery materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of ferric phosphate materials, and in particular to a titanium-doped anhydrous ferric phosphate material and a preparation method and application thereof, mainly a method for preparing titanium-doped anhydrous ferric phosphate with controllable titanium content by utilizing waste titanium element in titanium dioxide byproduct, which is beneficial to the preparation of battery materials. Background Art

[0002] Anhydrous iron phosphate is the precursor material of lithium iron phosphate, one of the current mainstream battery cathode materials; the process of preparing lithium iron phosphate by solid phase method is as follows Figure 1 As shown, it generally includes mixing, spray drying, sintering, pulverizing, mixing classification and baking processes. Figure 2 The conventional preparation process of iron phosphate is shown, which mainly uses iron solution, phosphorus solution and oxidant for oxidation synthesis, and obtains anhydrous iron phosphate through high-temperature crystallization, drying and calcination. In the modification research of iron phosphate battery materials, since both titanium and iron have d2sp3 hybridization mode, although the structure of the stable phase of titanium phosphate and iron phosphate is different, when titanium (Ti) is added to iron phosphate as a dopant, it can be arranged in the crystal according to the same rule as iron. It is generally believed that the modification effect of titanium doping on iron phosphate / lithium iron phosphate includes: ① Under the same unit cell parameter conditions, the smaller radius of titanium makes the electron migration channel wider; ② Due to the introduction of heterogeneous elements, the growth of crystals is hindered after nucleation, which can effectively reduce its primary particles, which is manifested in the electrical properties that the high rate performance of the prepared battery is significantly improved and the impedance is significantly reduced.

[0003] Among them, the doping nodes of titanium element can be divided into: ①Introduction during the solid phase method of lithium iron phosphate production; ②Introduction during the production of iron phosphate. The first type usually uses rutile titanium dioxide with better reaction activity to react with other materials at high temperature in the solid phase, but this reaction process requires a lot of heat energy and uninterrupted mechanical grinding.

[0004] Titanium is used as an alternative doping element to iron. It is introduced in the form of ions during the preparation of the second type of iron phosphate. There is almost no increase in energy consumption during the production process, which is a more ideal doping method, but there are many influencing factors. In the preparation of iron phosphate compounds, ferrous sulfate heptahydrate, a by-product of titanium dioxide, is generally used as the source of iron. Since this by-product is crystallized from the acid hydrolysis solution of ilmenite, it will be attached with a certain amount of titanium. Most companies that use this route to produce iron phosphate will remove this part of the titanium element by increasing the pH (adding alkali or reacting elemental iron with acid) when preparing the iron source solution. Under this route, it is necessary to further add titanium-containing materials to prepare titanium-doped iron phosphate products, and the quality of the product needs to be further improved. Summary of the invention

[0005] In view of the technical problems existing in the background technology, the present invention provides a titanium-doped anhydrous iron phosphate material and a preparation method and application thereof. The titanium-doped anhydrous iron phosphate material provided by the present invention has good performance quality, is easy to prepare, and is conducive to application in battery materials.

[0006] In a first aspect, an embodiment of the present invention provides a method for preparing a titanium-doped anhydrous ferric phosphate material, which comprises the following steps:

[0007] Providing titanium-containing ferrous sulfate raw material liquid and titanium-free ferrous sulfate raw material liquid;

[0008] Mixing the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid to obtain a mixed solution;

[0009] The mixed solution is mixed with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate;

[0010] The slurry is sequentially aged, rinsed, dried and sintered to obtain a titanium-doped anhydrous iron phosphate material.

[0011] In the technical solution of the embodiment of the present application, the titanium-containing ferrous sulfate raw material liquid is mixed with the titanium-free ferrous sulfate raw material liquid to obtain the mixed solution, and then the obtained mixed solution and the phosphorus source are oxidized to obtain a slurry containing iron phosphate and titanium phosphate, and then the slurry is aged, rinsed, dried, and sintered in sequence to obtain the titanium-doped anhydrous iron phosphate material. Among them, by mixing the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid in a certain proportion, the doping control of the titanium element in the final doped iron phosphate product can be achieved by adjusting the proportion, so that the titanium content in the prepared titanium-doped anhydrous iron phosphate material is stable and controllable, and then the problem of uncontrollable titanium content in anhydrous iron phosphate caused by uneven quality of ferrous sulfate heptahydrate can be solved; at the same time, the titanium-doped anhydrous iron phosphate prepared in this embodiment has a uniform nano-scale particle stacking morphology, which is conducive to application.

[0012] In some embodiments, the raw materials for preparing the titanium-containing ferrous sulfate raw material solution and the titanium-free ferrous sulfate raw material solution include titanium dioxide by-product, and the mass fraction of titanium in the titanium dioxide by-product is 600-4200 ppm.

[0013] In this embodiment, the titanium dioxide by-product is used when selecting the titanium element introduction source. The main component of the titanium dioxide by-product is ferrous sulfate heptahydrate, and titanium is attached to it, so no additional titanium needs to be added. At the same time, in the titanium dioxide by-product, the titanium element exists stably in the form of ions, which is beneficial to improving the quality of the prepared titanium-doped anhydrous ferric phosphate and also realizes waste utilization.

[0014] In addition, the titanium dioxide by-product having a titanium mass fraction in the range of 600-4200 ppm can be used as a raw material for the preparation of the titanium-doped anhydrous ferric phosphate material. In this embodiment, there are no excessive restrictions on the source of the titanium dioxide by-product.

[0015] In some embodiments, the steps of preparing the titanium-containing ferrous sulfate raw material solution include:

[0016] Dissolving the titanium dioxide byproduct with an acidic aqueous solution, and obtaining the titanium-containing ferrous sulfate raw material liquid after solid-liquid separation;

[0017] And / or, the steps of preparing the titanium-free ferrous sulfate raw material solution include:

[0018] The titanium dioxide byproduct is mixed with a phosphorus-containing solution, and after solid-liquid separation, the titanium-free ferrous sulfate raw material solution is obtained;

[0019] Wherein, the phosphorus-containing solution includes at least one of phosphoric acid or phosphate; the mass fraction of phosphorus element in the phosphorus-containing solution is 1000-3000 ppm.

[0020] In this embodiment, during the preparation of the titanium-containing ferrous sulfate raw material liquid, an acidic aqueous solution is used to dissolve the titanium dioxide by-product, and the acidic environment can keep the titanium element from hydrolyzing. During the preparation of the titanium-free ferrous sulfate raw material liquid, a phosphorus-containing solution is used to dissolve the titanium dioxide by-product to hydrolyze the titanium element.

[0021] In some embodiments, the pH values ​​of the titanium-containing ferrous sulfate raw material solution and the titanium-free ferrous sulfate raw material solution are 0.8-1.8, respectively.

[0022] In this embodiment, by controlling the pH values ​​of the titanium-containing ferrous sulfate raw material solution and the titanium-free ferrous sulfate raw material solution to be between 0.8 and 1.8, it is advantageous to obtain a slurry containing iron phosphate and titanium phosphate through the reaction.

[0023] In some embodiments, in the step of obtaining a slurry containing iron phosphate and titanium phosphate, the mixed solution is mixed with the oxidant and the phosphorus source according to a molar ratio of iron element, phosphorus element and oxidant of 1:1.01-1.05:0.55-0.65.

[0024] In this embodiment, the mixed oxidation is sufficient by adopting this ratio, and the prepared slurry containing iron phosphate and titanium phosphate has a high content of active substances.

[0025] In some embodiments, the steps of aging, rinsing, drying and sintering the slurry in sequence include:

[0026] The slurry is heated to 80-98° C. and kept warm for 1-4 hours, and then rinsed with water to obtain a phosphorus-containing rinse liquid and a filter cake;

[0027] The filter cake is dried and then sintered at 550-750° C. for 1-4 hours to obtain the titanium-doped anhydrous ferric phosphate material.

[0028] In this embodiment, the phosphorus-containing rinse liquid can be used to prepare titanium-free ferrous sulfate raw material liquid. On the one hand, it realizes the recycling of waste liquid and saves the cost of alkaline reagents. The ferrous solution not consumed in the preparation process of titanium-doped anhydrous ferric phosphate can also be used for the preparation of conventional ferric phosphate without waste. On the other hand, it can achieve impurity removal under the required low pH conditions, which is different from the increase of pH value by alkaline reagents.

[0029] In the second aspect, an embodiment of the present invention provides a titanium-doped anhydrous iron phosphate material, which is prepared by the preparation method described above; the titanium-doped anhydrous iron phosphate material has an anhydrous iron phosphate crystal structure and a nanoscale particle stacking morphology, wherein the Ti doping amount of the titanium-doped anhydrous iron phosphate material is less than or equal to 2wt%.

[0030] In the technical solution of the embodiment of the present invention, the titanium content in the prepared titanium-doped anhydrous iron phosphate material is stable, and its crystal structure is consistent with that of anhydrous iron phosphate. The Fe / P molar ratio of the titanium-doped anhydrous iron phosphate material is 0.96-1.01, and it has a nanoscale particle stacking morphology and a uniform material morphology, which is convenient for subsequent product applications.

[0031] In some embodiments, the Ti doping amount of the titanium-doped anhydrous iron phosphate material is less than or equal to 1wt%; in some embodiments, the Fe / P molar ratio of the titanium-doped anhydrous iron phosphate material is 0.96-1.01, and the specific surface area can be 8-10m 2 / g, the material properties are more conducive to subsequent applications.

[0032] In a third aspect, an embodiment of the present application provides a positive electrode plate, in which the titanium-doped lithium iron phosphate prepared from the titanium-doped anhydrous iron phosphate material described above is used as an active material.

[0033] In this embodiment, the titanium-doped anhydrous iron phosphate material can be used as a precursor to prepare an iron phosphate-based positive electrode material. The positive electrode material is prepared from the titanium-doped anhydrous iron phosphate and an ion battery source, specifically a titanium-doped lithium iron phosphate active material, and thus has the advantages of stable quality and good performance. The positive electrode battery material of this embodiment is used to assemble and prepare a battery pole piece and its device with corresponding good performance.

[0034] In a fourth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate described above.

[0035] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of stable quality and good performance.

[0036] In a fifth aspect, an embodiment of the present application provides an electrical device, comprising the secondary battery described above.

[0037] In this embodiment, the electrical device includes the secondary battery, and thus has the advantages of stable quality and good performance.

[0038] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only part of the embodiments or some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0040] Figure 1 The process of preparing lithium iron phosphate by the existing solid phase method;

[0041] Figure 2 This is a conventional preparation process for iron phosphate;

[0042] Figure 3 A schematic diagram of the process for preparing titanium-doped anhydrous ferric phosphate materials according to some embodiments of the present invention;

[0043] Figure 4 The XRD pattern of the final product sample of Example 1 of the present invention;

[0044] Figure 5 This is a SEM image of the final product sample of Example 1 of the present invention. DETAILED DESCRIPTION

[0045] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0047] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0048] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0049] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0050] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0051] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0052] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0053] At present, there are two main ways to dope titanium: ① Exogenous introduction, adding titanium-containing materials; ② When preparing and producing iron phosphate, the iron source material is often ferrous sulfate heptahydrate, a byproduct of titanium dioxide, which itself is attached with some residual ilmenite extract during crystallization and separation. This part of titanium can be introduced into anhydrous iron phosphate. The first path requires the addition of a raw material and a raw material addition step. At the same time, because the design value of the titanium content in the final product is often less than 1%, it is difficult for titanium to exist stably in an aqueous solution. If hydrolysis occurs, it will be difficult to reverse. The subsequent doping form also changes from iron position substitution to solid phase mixing, which makes the feeding method difficult to design. For example, CN111908441A uses a mixed solution of ferrous sulfate, iron filings and phosphoric acid as the base liquid, introduces a titanium salt solution from an external source, forms titanium phosphate, and then drips hydrogen peroxide and alkali to precipitate the iron phosphate and form a coating on the titanium phosphate.

[0054] The second route does not require any new raw materials, has cost advantages, and can reduce the amount of waste residue generated during the production of iron salts, turning waste into treasure, which is more in line with the concept of energy conservation and emission reduction. However, it also has the defect of unstable content, because different titanium dioxide manufacturers have different treatment methods and limits for by-products, resulting in different pH, titanium content, and main content of solid ferrous sulfate heptahydrate. Since titanium has amphoteric properties and is very easy to form metatitanic acid, it is often necessary to retain all soluble titanium when retaining titanium in solid ferrous iron. At the same time, since iron phosphate is obtained by liquid phase precipitation, insoluble titanium precipitates need to be filtered out when iron salts are made. These reasons lead to the titanium element doped into anhydrous iron phosphate being completely affected by ferrous sulfate heptahydrate. Therefore, manufacturers that currently produce titanium-containing iron phosphate in this way only use solid ferrous iron provided by the same titanium dioxide factory in order to stabilize the titanium content in anhydrous iron phosphate.

[0055] In order to solve the technical problems of the prior art of adding titanium-containing materials for preparation or high energy consumption, and the product quality needs to be improved, the present invention first provides a method for preparing titanium-doped anhydrous ferric phosphate material, which comprises the following steps:

[0056] S1. Providing titanium-containing ferrous sulfate raw material liquid and titanium-free ferrous sulfate raw material liquid;

[0057] S2, mixing the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid to obtain a mixed solution;

[0058] S3, mixing the mixed solution with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate;

[0059] S4. The slurry is aged, rinsed, dried and sintered in sequence to obtain a titanium-doped anhydrous iron phosphate material.

[0060] Specifically, in step S1, a titanium-containing ferrous sulfate raw material liquid (hereinafter referred to as the first ferrous solution) and a titanium-free ferrous sulfate raw material liquid (hereinafter referred to as the second ferrous solution) need to be provided, wherein the first ferrous solution is obtained by dissolving the titanium dioxide by-product in an acidic aqueous solution and separating the solid from the liquid; the second ferrous solution is obtained by mixing the titanium dioxide by-product with a phosphorus-containing solution and separating the solid from the liquid, and the phosphorus-containing solution includes at least one of phosphoric acid or phosphates.

[0061] Wherein, the raw materials for preparing the first ferrous solution and the second ferrous solution are preferably titanium dioxide byproducts, the main component of which is ferrous sulfate heptahydrate, and at the same time, it also contains a small amount of titanium element, generally in the form of solid powder or powder. For the selection of titanium dioxide byproducts, any material available on the market can be used, wherein the titanium content is 600-4200ppm (mass fraction, parts per million) as the preferred range, and more preferably 2000-4000ppm. It should be noted that titanium dioxide byproducts usually also contain very few metal element impurities such as aluminum, potassium, magnesium, and manganese. For example, the main content of titanium dioxide byproducts (in terms of ferrous sulfate heptahydrate) is ≥80%, preferably ≥85%; the pH value (10g solid dissolved in 100g water) is 2.5-3.25; in addition, the cationic impurity indicators are: lead (Pb) <20ppm, nickel (Ni) <100ppm, chromium (Cr) <65ppm, copper (Cu) <20ppm, zinc (Zn) <100ppm.

[0062] Further, in this embodiment, the titanium dioxide byproduct is dissolved in an acidic aqueous solution, and after solid-liquid separation, a first ferrous solution is obtained. For example, concentrated sulfuric acid can be diluted with water to a dilute sulfuric acid solution, stirred for 5-10 minutes to ensure uniformity, and then the titanium dioxide byproduct is added and stirred for 10-15 minutes to disperse and dissolve uniformly. Among them, the weight ratio of the titanium dioxide byproduct to water can be 1:1.0-2.0; the molar ratio of the titanium dioxide byproduct to the added sulfuric acid can be 32-40:1, and the pH value of the obtained first ferrous solution should be 0.8-1.8. Preferably, a filter press is used for solid-liquid separation to separate foreign matter such as dust, sediment, plastic film, and insoluble compounds (mainly titanate) carried in the solid ferrous iron. The filtered first ferrous solution contains titanium ions, sulfate ions, ferrous ions, etc.

[0063] Furthermore, in this embodiment, the titanium dioxide byproduct is mixed with a phosphorus-containing solution, and after solid-liquid separation, a second ferrous solution is obtained. The components of the phosphorus-containing solution include one or more of phosphoric acid and phosphates. Preferably, a phosphorus-containing rinse liquid (or phosphoric acid, ammonium phosphate, sodium phosphate, etc.) is mixed with water to prepare a phosphorus-containing solution with a phosphorus mass fraction of 1000ppm-3000ppm. Specifically, in the embodiment of the present invention, the phosphorus-containing solution is added to the reactor, and after stirring, the titanium dioxide byproduct powder is added to the reactor. The mass ratio of the titanium dioxide byproduct to the phosphorus-containing solution is 1:1.0-2.0; after the addition is completed, it can be stirred for 10-15min to react evenly, involving the reaction: 3Ti 4+ +4PO4 3- →Ti3(PO4)4; the pH value of the obtained second ferrous solution should be between 0.8 and 1.8. After the reaction is completed, solid-liquid separation is performed to obtain a ferrous solution free of titanium, namely the second ferrous solution.

[0064] During the preparation of the above-mentioned first ferrous solution, the acidic environment can keep the titanium element from hydrolyzing; during the preparation of the second ferrous solution, it is preferred to use the phosphorus-containing rinsing liquid and pure water in the preparation process of ferric phosphate to prepare the dissolving solution, which not only recycles the waste liquid, but also ensures a lower pH value of the ferrous solution after impurities are removed, and can avoid the risk of hydrolysis of the titanium element during subsequent mixing to prepare the second ferrous solution.

[0065] In step S2, the first ferrous solution and the second ferrous solution are mixed to obtain a mixed solution. In this embodiment, by adjusting the mixing ratio of the first ferrous solution and the second ferrous solution, a controllable design of the titanium content in the final product within the range of 0-2% can be achieved, which is convenient for solving the problem of uncontrollable titanium content in anhydrous ferric phosphate caused by uneven quality of ferrous sulfate heptahydrate. For example, the first ferrous solution and the second ferrous solution can be mixed in a mass ratio of 4:1 or 1:4.

[0066] Specifically, in step S3, the mixed solution is mixed with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate. In this embodiment, a phosphorus source is also prepared by preparing a phosphorus-containing material and water into a solution with a phosphorus mass fraction of 6-18%, and the phosphorus-containing material includes but is not limited to phosphoric acid, ammonium phosphate, sodium phosphate, etc.

[0067] In step S3, in this embodiment, stirring can be turned on during the process of mixing the mixed solution with the oxidant and the phosphorus source. The stirring frequency is related to the stirring equipment and the reaction volume, and it is in accordance with the principle of sufficient dispersion and no splashing out of the reaction container. For example, the oxidant (commonly used hydrogen peroxide) and the phosphorus source are added to the mixed solution at the same time, and the dropping time is controlled at 20-60min. Here, the proportion of each material is calculated according to the amount of substance, and the molar ratio is preferably n iron element: n phosphorus element (P): n hydrogen peroxide (H2O2) = 1: 1.01-1.05: 0.55-0.65; this reaction method can ensure that the titanium element is evenly dispersed in the slurry. After the dropwise addition is completed, the present embodiment can obtain a yellow slurry, and the yellow slurry contains the generated iron phosphate and titanium phosphate.

[0068] Reactions include:

[0069] 2Fe 2+ +H2O2+HPO4 2- +H2PO4 - →2FePO4↓+2H2O+H + ;

[0070] 3Ti 4+ +4PO4 3- →Ti3(PO4)4.

[0071] Specifically, in step S4, the slurry is aged, rinsed, dried and sintered in sequence; wherein, in this embodiment, the aging can be carried out under stirring conditions to achieve crystal transformation. The obtained slurry is preferably heated to 80-98°C (more preferably 92-95°C) in a kettle, and kept warm for 1h-4h to achieve high-temperature crystal transformation, and filtered after the insulation is completed.

[0072] In step S4, 10-30% of phosphoric acid of the amount of iron phosphate material can be added during the aging process to accelerate the conversion rate. After aging, rinsing is also included, in which the impurities in the slurry precipitation are removed by water washing, and filtered to obtain a precipitate and a phosphorus-containing rinsing liquid (which can be rinsed until the conductivity of the newly filtered rinsing water is not higher than 200μs / cm); the phosphorus-containing rinsing liquid is used to provide a titanium-free ferrous sulfate raw material liquid, that is, it can be recovered and used for the preparation of a phosphorus-containing solution. The embodiment of the present invention can use the phosphorus-containing rinsing liquid to prepare the above-mentioned second ferrous solution, which can not only maintain the low pH value of the solution, but also realize the secondary utilization of the waste liquid.

[0073] In step S4, the filter cake is dried, and the drying is preferably carried out in a baking manner, that is, the rinsed filter cake is dried and water is controlled, and sintered at 550-750°C for 1-4h, and the heating rate can be controlled to be 3-5°C / min. After the sintering is completed, the product titanium-doped anhydrous iron phosphate material is obtained.

[0074] Furthermore, combined with Figure 3The flow chart of the preparation of titanium-doped anhydrous iron phosphate material shows the contents. In the embodiment of the present invention, firstly, ferrous sulfate heptahydrate, sulfuric acid and water are used to prepare a first ferrous solution, and ferrous sulfate heptahydrate and a phosphorus-containing solution are used to prepare a second ferrous solution. Secondly, the first ferrous solution and the second ferrous solution are mixed to obtain a mixed solution. Then, the mixed solution is mixed with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate. Finally, the obtained slurry is aged and rinsed in turn, and a filter cake and a phosphorus-containing rinse liquid are obtained after rinsing. The obtained filter cake is dried and sintered in turn to prepare a titanium-doped anhydrous iron phosphate material; and the phosphorus-containing rinse liquid and water are used to prepare a phosphorus-containing solution, which is reused as the ingredient of the second ferrous solution. The yield of the titanium-doped iron phosphate prepared in the embodiment of the present invention is above 99%, and the titanium element in the titanium dioxide byproduct ferrous sulfate heptahydrate can be recycled, thereby reducing waste and reducing raw materials, and turning waste into treasure. The method of the present invention can obtain anhydrous iron phosphate doped with titanium, which has good performance and quality, and low energy consumption for preparation.

[0075] Secondly, an embodiment of the present invention provides a titanium-doped anhydrous iron phosphate material, which is prepared by the preparation method described above, has an anhydrous iron phosphate crystal structure, and has a nanoscale particle stacking morphology. The Fe / P molar ratio of the titanium-doped anhydrous iron phosphate material is 0.96~1.01, and the Ti doping amount is less than or equal to 2wt%.

[0076] In some embodiments of the present invention, the titanium-doped anhydrous ferric phosphate material has a Ti doping amount less than or equal to 1 wt%, and can be prepared by the preparation method described above. In addition, the titanium-doped anhydrous ferric phosphate material can have a specific surface area of ​​8 to 10 m 2 / g.

[0077] The titanium content in the finished product of the titanium-doped anhydrous ferric phosphate material described in the embodiment of the present invention is stable, its crystal structure is consistent with that of anhydrous ferric phosphate (according to X-ray diffraction pattern analysis), and it has a nanoscale particle stacking morphology (according to scanning electron microscope image analysis). The sample material has a uniform morphology, which is convenient for subsequent product applications.

[0078] Furthermore, the embodiments of the present invention also provide the use of the titanium-doped anhydrous iron phosphate material described above in the preparation of electrode materials and batteries, specifically positive electrode plates, secondary batteries and electrical devices. The titanium-doped anhydrous iron phosphate material can be used as a precursor to prepare iron phosphate positive electrode materials, and the positive electrode material is prepared from the above-mentioned titanium-doped anhydrous iron phosphate and an ion battery source (such as lithium salt). The positive electrode battery material of this embodiment is used to assemble and prepare the corresponding battery plates and their devices and apparatus. The preparation of the electrode materials and batteries described in the embodiments of the present invention is a conventional preparation method in the field. Through the preparation of precursor materials, the technical effect of stable quality can be achieved, and the performance of positive electrode plates, secondary batteries and electrical devices can also be improved.

[0079] In some embodiments of the present application, the secondary battery can be used as an operating power source, a driving power source, etc. of an electrical device; it can include multiple battery cells, and the multiple battery cells can be connected in series, in parallel, or in mixed connection. The battery cell can be cylindrical, flat, rectangular, or in other shapes. The secondary battery can also include a busbar component for realizing electrical connection between the multiple battery cells.

[0080] The electric device provided in the embodiment of the present application may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0081] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.

[0082] Embodiment 1,

[0083] 1. Preparation of the first ferrous solution: Add 7kg of pure water to the reactor, then add 50g of concentrated sulfuric acid (75%wt) to dilute, stir for 10min, add 3.5kg of ferrous sulfate heptahydrate and stir for 15min. Here, ferrous sulfate heptahydrate is a byproduct of titanium dioxide sold by Longmang Group (see the table below for ingredients). After the dispersion and dissolution is completed, the pH value of the solution is measured to be 1.707, and the solution after filtration is the first ferrous solution.

[0084] Table 1 Titanium dioxide by-product detection results

[0085]

[0086] 2. Preparation of phosphorus-containing solution and second ferrous solution: 20 kg of phosphorus-containing rinse liquid collected from a workshop of a certain ferric phosphate company in Hubei Province was mixed with 10 kg of pure water to prepare a phosphorus-containing solution; 7 kg of phosphorus-containing solution was added to a reactor, and after stirring, 3.5 g of ferrous sulfate heptahydrate was added to the reactor, where ferrous sulfate heptahydrate is a byproduct of titanium dioxide sold by Longmang Group, and the reaction was stirred for 10-15 minutes, and the pH value was measured to be 1.401. Filter to obtain a second ferrous solution.

[0087] 3. Preparation of phosphorus source: Dissolve 5 kg of ammonium dihydrogen phosphate in 16 kg of pure water, add 3 kg of ammonia water and stir thoroughly to obtain a phosphorus source. (The materials in steps 1, 2, and 3 are all in excess and are used for other examples and comparative examples)

[0088] 4. Preparation of mixed solution: Mix the first ferrous solution and the second ferrous solution in a mass ratio of 4:1, and stir for 10 minutes to obtain 750g of mixed solution.

[0089] 5. Preparation of titanium-doped ferric phosphate: 60 g of hydrogen peroxide and 355.96 g of phosphorus-containing solution A were simultaneously added dropwise to 750 g of the mixed solution. The addition time was controlled within 40 min. After the addition was completed, a yellow slurry was obtained.

[0090] 6. Crystal transformation (aging): Keep stirring, add 10 g of 86% wt phosphoric acid to the slurry, heat to 95° C. and keep warm for 2 hours, and obtain a white slurry after the insulation is completed.

[0091] 7. Rinse and remove impurities: remove impurities in the slurry precipitation by water washing, rinse until the conductivity of the newly filtered rinsing water is not higher than 200μs / cm, and obtain phosphorus-containing rinsing liquid and filter cake.

[0092] 8. Drying and sintering: The rinsed filter cake was dried at 98°C for 6 hours, and then sintered in a muffle furnace at 700°C for 2 hours. The heating rate was controlled at 4°C / min. After sintering, 114.87 g of anhydrous iron phosphate was obtained.

[0093] Figure 4 , Figure 5 The X-ray diffraction (XRD) pattern and scanning electron microscope (SEM) image of the final product sample of Example 1 of the present invention are compared with the diffraction peak angle in the XRD pattern and the standard card 29-0715, and it can be confirmed that the crystal structure of the sample is consistent with anhydrous ferric phosphate. The SEM image shows that the sample of Example 1 of the present invention is formed by melting and stacking nano-scale particles.

[0094] Embodiment 2,

[0095] The first ferrous solution and the second ferrous solution in Example 1 are still used, but the mixing ratio of the two ferrous solutions in step 3 is adjusted to 1:4. The remaining steps are exactly the same.

[0096] Embodiment 3,

[0097] The source of ferrous sulfate heptahydrate in step 1 was changed from that sold by Lomon Group to titanium dioxide byproduct sold by Billions Group to prepare the first ferrous solution, and the subsequent steps were the same as in Example 1. The second ferrous solution was prepared using the titanium dioxide byproduct sold by Lomon Group as raw material.

[0098] Embodiment 4,

[0099] The source of ferrous sulfate heptahydrate in step 2 was changed to the titanium dioxide byproduct sold by Billions Group to prepare the second ferrous solution, and the other steps were the same as in Example 1. The raw material for preparing the first ferrous solution was still the titanium dioxide byproduct sold by Lomon Group.

[0100] Table 2 Detection results of titanium dioxide byproducts in Example 4

[0101]

[0102] Comparative Example 1

[0103] The first ferrous solution in Example 1 is still used, but the mixed solution in step 3 is changed to completely use the first ferrous solution.

[0104] Comparative Example 2

[0105] When preparing the first ferrous solution in step 1, sulfuric acid is not added for dilution, and the other steps are the same as those in Example 1.

[0106] Comparative Example 3

[0107] When preparing the second ferrous solution in step 2, the method for preparing the phosphorus-containing solution B is not used, 1 kg of ferrous sulfate heptahydrate is dissolved in 2 kg of water, and sodium hydroxide is used to adjust the pH value to 3. The other steps are the same as in Example 1.

[0108] The samples obtained in each embodiment and comparative example were tested and characterized, and the equipment and methods included: 1. Specific surface area (BET) detection: TristarⅡ3020 specific surface area detector; 2. Metal element content: 5110ICP-OES spectrometer; 3. Iron element: GB / T6730.66-2009; 4. Phosphorus element: quinoline molybdate gravimetric method. The test data BET, Fe / P content are shown in Table 3, and the battery-grade iron phosphate restricted metal element content is shown in Table 4.

[0109] Table 3 BET and Fe / P contents of samples obtained from examples and comparative examples

[0110]

[0111]

[0112] Table 4 Restricted metal element content of battery-grade iron phosphate

[0113]

[0114] Compare the data in Table 3: Due to the small amount of titanium doping, there is no obvious change in the specific surface area, and there is a slight effect on the molar ratio of iron and phosphorus. The more titanium, the lower the ratio, because titanium will replace iron.

[0115] Compare the mass fractions of metal element impurities in Table 4:

[0116] ① Compared with Comparative Example 1, when Example 1 is prepared, the ratio of the first ferrous solution and the second ferrous solution is changed, so the titanium content in the sample also changes accordingly. When the mixing ratio is 4:1, the titanium content is 2356.04ppm, and when the ratio is 5:0, it is 2898.26ppm. Compared with Example 2, the mixing ratio of Example 2 is 4:1, and the titanium content in the sample is 603.8ppm. Comprehensive comparison shows that the maximum amount of titanium doped in iron phosphate produced by dissolving this batch of ferrous sulfate heptahydrate and pure water in a ratio of 1:2 is about 2898ppm. When the first ferrous solution and the second ferrous solution are mixed in different proportions, anhydrous iron phosphate samples with corresponding titanium content can be obtained.

[0117] ② In comparison between Example 1 and Example 3, the source of the titanium dioxide byproduct of the first ferrous solution was changed, and the titanium content in the sample also changed. The titanium content of the sample in Example 3 was 4189.46 ppm, indicating that the maximum titanium content of the present invention is related to the source of the raw materials of the first ferrous solution. This is because the source of the titanium element in the present invention is the attached titanium of ferrous sulfate heptahydrate in the first ferrous solution, so the maximum content is affected by it.

[0118] ③Comparing Example 1 with Example 4, the source of the byproduct of titanium dioxide in the preparation of the second ferrous solution was changed, and the final samples had no difference. This is because the use of phosphorus-containing solution B can remove impurities from the second ferrous solution, so it has no effect on the sample composition. The second ferrous solution only plays a role in adjusting the titanium content and is not affected by the source of the raw materials.

[0119] ④ In Comparative Example 2, sulfuric acid was not added to control the pH when the first ferrous solution was prepared. Compared with Example 1, the titanium content in the final sample decreased. This is because the pH of pure water used to dissolve the first ferrous solution was relatively high (the measured data was 2.1), which caused some titanium ions to hydrolyze to form colloids, which were intercepted during filtration.

[0120] ⑤ In comparative example 3, the preparation method of the second ferrous solution was changed to pure water dissolution and the pH was increased to control impurities. In both tests, the aluminum impurity content was only less than 20% of that of other samples, but the detected titanium element was not parallel, indicating that the distribution of titanium element in the sample was not uniform. This is because when the first ferrous solution and the second ferrous solution were mixed, part of the titanium ions were hydrolyzed due to the increase in pH. Although the hydrolysis in this step would not reduce the titanium element, the colloid formed would make the titanium element insufficiently dispersed. After the sintering step, the final form of this part of the titanium element was only amorphous titanate or titanium dioxide.

[0121] As can be seen from the above embodiments, the present invention uses a titanium-containing ferrous sulfate raw material liquid (preferably prepared from a titanium dioxide byproduct) to carry out a batching step with a titanium-free ferrous sulfate raw material liquid, and then the obtained mixed solution and a phosphorus source are oxidized to obtain a slurry containing iron phosphate and titanium phosphate, and then aged, rinsed, dried, and sintered in sequence to obtain a titanium-doped anhydrous ferric phosphate material. The present invention mainly adjusts the addition of ferrous solution to two stages, and the doping control of the titanium element in the final doped ferric phosphate product can be achieved by adjusting the proportion, thereby making the titanium content in the finished product stable and controllable; at the same time, the titanium-doped anhydrous ferric phosphate product has a uniform nano-scale particle stacking morphology, which is conducive to the application of preparing battery materials. In addition, the present invention is simple to prepare and has low energy consumption. The titanium attached to the titanium dioxide byproduct ferrous sulfate heptahydrate itself can be used. Before the reaction, the titanium element is stably present in the form of ions, which can not only improve the quality of the finished product, but also realize waste utilization.

[0122] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for preparing titanium-doped anhydrous ferric phosphate material, It is characterized in that Includes steps: Providing titanium-containing ferrous sulfate raw material liquid and titanium-free ferrous sulfate raw material liquid; Mixing the titanium-containing ferrous sulfate raw material liquid and the titanium-free ferrous sulfate raw material liquid to obtain a mixed solution; The mixed solution is mixed with an oxidant and a phosphorus source to obtain a slurry containing iron phosphate and titanium phosphate; The slurry is sequentially aged, rinsed, dried and sintered to obtain a titanium-doped anhydrous iron phosphate material; The steps for preparing the titanium-containing ferrous sulfate raw material solution include: Dissolving the titanium dioxide byproduct in an acidic aqueous solution, and obtaining the titanium-containing ferrous sulfate raw material liquid after solid-liquid separation; And / or, the steps of preparing the titanium-free ferrous sulfate raw material solution include: The titanium dioxide byproduct is mixed with the phosphorus-containing solution, and after solid-liquid separation, the titanium-free ferrous sulfate raw material liquid is obtained; The phosphorus-containing solution includes at least one of phosphoric acid or phosphate; the mass fraction of phosphorus in the phosphorus-containing solution is 1000-3000 ppm; the pH values ​​of the titanium-containing ferrous sulfate raw material solution and the titanium-free ferrous sulfate raw material solution are both 0.8-1.

8.

2. The preparation method according to claim 1, It is characterized in that The raw materials for preparing the titanium-containing ferrous sulfate raw material solution and the titanium-free ferrous sulfate raw material solution include titanium dioxide by-product, and the mass fraction of titanium in the titanium dioxide by-product is 600-4200 ppm.

3. The preparation method according to any one of claims 1 to 2, It is characterized in that In the step of obtaining the slurry containing iron phosphate and titanium phosphate, the mixed solution is mixed with the oxidant and the phosphorus source according to a molar ratio of iron element, phosphorus element and oxidant of 1:1.01-1.05:0.55-0.

65.

4. The preparation method according to any one of claims 1 to 2, It is characterized in that The steps of sequentially aging, rinsing, drying and sintering the slurry include: The slurry is heated to 80-98° C. and kept warm for 1-4 hours, and then rinsed with water to obtain a phosphorus-containing rinse liquid and a filter cake; The filter cake is dried and then sintered at 550-750° C. for 1-4 hours to obtain the titanium-doped anhydrous ferric phosphate material.

5. A titanium-doped anhydrous iron phosphate material, It is characterized in that Prepared by the preparation method described in any one of claims 1-4; the titanium-doped anhydrous iron phosphate material has an anhydrous iron phosphate crystal structure and a nano-scale particle stacking morphology, wherein the Ti doping amount of the titanium-doped anhydrous iron phosphate material is less than or equal to 2wt%.

6. A positive electrode sheet, It is characterized in that The titanium-doped lithium iron phosphate prepared from the titanium-doped anhydrous iron phosphate material as claimed in claim 5 is used as the active material.

7. A secondary battery, It is characterized in that Including the positive electrode sheet as described in claim 6.

8. An electrical device, It is characterized in that A secondary battery comprising the secondary battery according to claim 7.

Citation Information

Cited By

  • Method for preparing low-aluminum titanium-doped iron phosphate material by utilizing ferrophosphorus slag

    CN120246954A