A star-shaped polyaryletherketone resin TS-PEKK, its preparation method and uses
By using triphenyl oxybenzene (TPOB) as a branching agent, star-shaped polyaryletherketone resin TS-PEKK was prepared, which solved the problems of high glass transition temperature and high melting temperature of polyaryletherketone resin. It also achieved good solubility in low-toxicity solvents and melt thermal oxidation stability, making it suitable for the preparation of composite materials.
Patent Information
- Application Number
- CN202310558932.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-30
- Filing Date
- 2023-05-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-17
AI Technical Summary
Existing polyaryletherketone resins have high glass transition temperatures and high melting temperatures, making them difficult to process and mold. They also lack sufficient solubility and melt thermal oxidative stability in common low-toxicity organic solvents.
Star-shaped polyaryletherketone resin TS-PEKK was prepared by electrophilic polymerization of triphenoxybenzene (TPOB) with aryl ethers and aryl diacyl chlorides in a catalyst solvent system, using TPOB as a branching agent. The performance of the resin was optimized by controlling the molar ratio and reaction conditions.
It increases the glass transition temperature of the resin, lowers the melting temperature, enhances its solubility in low-toxicity organic solvents and its melt thermal oxidation stability, simplifies the processing, and is suitable for the preparation of composite materials.
Smart Images

Figure CN117757040B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of special engineering plastics technology, specifically relating to a star-shaped polyaryletherketone resin TS-PEKK, its preparation method, and its uses. Technical Background
[0002] Polyaryletherketone (PEAK) resins are a class of thermoplastic polymers whose macromolecular backbone is composed of aromatic ether and aromatic ketone structural units. This unique structural characteristic endows them with excellent high and low temperature resistance, superior mechanical properties, dimensional stability, resistance to various media, weather resistance, flame retardancy, and resistance to nuclear radiation. They are particularly suitable as matrix resins for high-performance thermoplastic composites and super engineering plastics. They have wide applications in high-tech fields such as aerospace, microelectronics, information engineering, machinery manufacturing, medical devices, oil extraction, transportation, and weaponry, and have become an indispensable new material in modern high-tech fields.
[0003] There are two technical routes for the preparation of PEAK. One is the nucleophilic route, in which a nucleophilic substitution reaction occurs between a ketone-containing difluorinated monomer and a bisphenol (sodium, potassium) salt monomer in a high-boiling-point aprotic, highly polar organic solution to form an ether bond that links the aromatic ring skeleton into a linear polymer structure. The most typical examples are polyarylether ether ketone (PEEK), polyarylether ketone (PEK), and PEEKK. The other method is called the electrophilic route, in which an aryl diacyl chloride and an aryl ether undergo a Friedel-Crafts acylation reaction in the presence of anhydrous aluminum trichloride catalyst to form a ketone group that links the aromatic ring skeleton into a linear macromolecule. It can be seen that the type, structure, and purity of the monomer determine the structure, type, and properties of the polymer.
[0004] PEAK is mostly a crystalline polymer. Except for a very few strong protic acids such as concentrated H₂SO₄, it is insoluble in common organic solvents, and its melting temperature (T) is relatively high. m The glass transition temperature (T) is relatively high. g The value is relatively low. For example, PEEK's T... m The temperature was 343℃, T g The temperature is 143℃, and the T value of PEKK is... m 354℃, T g The glass transition temperature (Tm) of PEAK resin is 156℃. The melt processing temperature of PEAK resin is generally 30℃ to 60℃ higher than its Tm, which places high demands on processing equipment and processes, making processing difficult and limiting its application range. Therefore, molecular design is used to increase the glass transition temperature (Tm) of PEAK. g The research and development of polyaryletherketones (PAGEs) focuses on improving their melting temperature (Tm) while maintaining their high and low temperature resistance, as well as their solubility in some common low-toxicity organic solvents. Solvent-based processing is also a key area of research.
[0005] Hyperbranched polyaryletherketone (HBPEAK) not only possesses the excellent mechanical properties of linear polyaryletherketone resins, but also exhibits the melt flowability characteristic of hyperbranched polymers and a higher TL. g and lower T m The melt processing performance is significantly improved.
[0006] Patent application CN 107987272A uses 1,3,5-benzenetricarboxyl chloride, 1,2,4-benzenetricarboxyl chloride, and bis-(3,4-phthalic anhydride)benzophenone as branching agents, employing an electrophilic polymerization route, to co-condense with TPC, IPC, and diphenyl ether (DPE) to synthesize high molecular weight polyarylether ketones. While this method uses benzenetricarboxyl chloride and bis-(3,4-phthalic anhydride)benzophenone as branching agents to synthesize hyperbranched PEKK and can produce high molecular weight polymers, the branching agents are unstable, prone to hygroscopic deterioration, and cause side reactions under Friedel-Crafts acylation polycondensation conditions, resulting in insufficient melt thermal oxidative stability of the prepared HBPEKK.
[0007] Therefore, there is an urgent need for a polyarylether ketone with a high glass transition temperature, low melting temperature, good resistance to high and low temperatures, good solubility in common low-toxicity organic solvents, and good molten thermal oxidation stability, as well as its preparation method. Summary of the Invention
[0008] To address the above problems, the present invention provides the following technical solution.
[0009] In one aspect, a polyaryletherketone resin is provided.
[0010] A polyaryletherketone resin with the structure shown in Formula I.
[0011]
[0012] Wherein, A2 is an aramid structure;
[0013] B2 has an aromatic ether structure;
[0014] B3 is selected from:
[0015]
[0016] m, n, and p represent the degree of polymerization;
[0017] The aramid structure is as follows:
[0018]
[0019] The aromatic ether structure is as follows:
[0020]
[0021] One or more of the following;
[0022] The The molar ratio is (9-1):(1-9).
[0023] The polyaryletherketone resin is a star-shaped polyaryletherketone resin.
[0024] In some embodiments, the logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl to 1.25 g / dl.
[0025] In some embodiments, the aryl diacyl structure is:
[0026]
[0027] The aromatic ether structure is as follows:
[0028]
[0029] One or more of the following; in such embodiments, the resulting polyaryletherketone resin is referred to as TS-PEKK resin in this invention.
[0030] In some embodiments, the aryl diacyl structure is:
[0031]
[0032] The aromatic ether structure is as follows:
[0033]
[0034]
[0035] One or more of them, the The molar ratio is 1:9-9:1, 8:2-2:8, 7:3-3:7, 6:4, 5:5 or 4:6; in such embodiments, the resulting polyaryletherketone resin is referred to as TS-PEKK resin in this invention.
[0036] In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKKS resin is 0.50 g / dl-1.20 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKKS resin is 0.50 g / dl-0.91 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKKS resin is preferably 0.60 g / dl-0.86 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKKS resin is preferably 0.60 g / dl-0.78 g / dl.
[0037] Secondly, a method for preparing polyaryletherketone resin is provided.
[0038] A method for preparing a polyaryletherketone resin includes: reacting mesityleneoxybenzene, arylene ether and arylene diacyl chloride in a catalyst solvent system, followed by post-treatment to obtain the polyaryletherketone resin.
[0039] In some embodiments, a method for preparing the polyarylether ketone resin of the first aspect includes: mixing an aromatic ether with a catalyst solvent system to undergo a complexation reaction, then adding an aromatic diacyl chloride to carry out a Friedel-Crafts acylation reaction, then adding mestriphenoxybenzene to carry out a first reaction, and after post-treatment, obtaining the polyarylether ketone resin.
[0040] In some embodiments, the structure of the polyaryletherketone resin is as shown in Formula I of the first aspect.
[0041] In some embodiments, the logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl to 1.25 g / dl.
[0042] In some embodiments, the aramid chloride is
[0043]
[0044] The aromatic ether is:
[0045]
[0046] One or more of the following; in such embodiments, the resulting polyaryletherketone resin is TS-PEKK resin.
[0047] In some embodiments, the aramid chloride is
[0048] The aramid chloride is
[0049] The molar ratio of the feed is 1:9-9:1, 2:8-8:2, 7:3-3:7, 6:4, 5:5 or 4:6, preferably 3:7-7:3;
[0050] The aromatic ether is:
[0051]
[0052] One or more of the following; in such embodiments, the resulting polyaryletherketone resin is TS-PEKK resin.
[0053] In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-1.25 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-1.00 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-0.91 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is preferably 0.60 g / dl-0.88 g / dl.
[0054] In some embodiments, the molar ratio of the mesityleneoxybenzene to the aryl ether in the aforementioned TS-PEKK resin is (0.3-1.5):100.0.
[0055] In some embodiments, the molar ratio of the aromatic ether to the aromatic diacyl chloride in the aforementioned TS-PEKK resin is (1.00 to 1.05):1.00.
[0056] In some embodiments, the catalyst solvent system includes a diluent, a Lewis acid, a Lewis base, and a co-catalyst.
[0057] In some embodiments, the diluent comprises an aprotic organic solvent.
[0058] In some embodiments, the aprotic organic solvent includes one or more of dichloromethane (DCM), dichloroethane (DCE), chloroform, o-dichlorobenzene, and tetrachloroethane.
[0059] In some embodiments, the aprotic organic solvent includes one or more of dichloromethane, dichloroethane, and o-dichlorobenzene. In some embodiments, 0.10 mol to 0.80 mol of aryl dichlorochloride is added per 1 L of the diluent. In some embodiments, 0.30 mol to 0.70 mol of aryl dichlorochloride is added per 1 L of the diluent.
[0060] In some embodiments, the Lewis acid includes one or more of AlCl3, FeCl3, and InCl3. In some preferred embodiments, the Lewis acid is AlCl3.
[0061] In some embodiments, the molar amount of the Lewis acid is the total molar amount of carbonyl, ketone, amide, and sulfone groups in the feedstock during the complexation reaction, plus the molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction, wherein the molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction is 0.5 to 2.2 times the molar amount of the aramid chloride. In some embodiments, the molar amount of the Lewis acid is the total molar amount of carbonyl, ketone, amide, and sulfone groups in the feedstock during the complexation reaction, plus the molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction, wherein the molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction is 0.5 to 1.0 times the molar amount of the aramid chloride.
[0062] In some embodiments, the Lewis base includes one or more of N-dimethylformamide (DMF), N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), sulfolane, and diphenyl sulfone.
[0063] In some embodiments, the cocatalyst comprises an organic acid salt or an inorganic acid salt.
[0064] In some embodiments, the co-catalyst comprises Fe 2+ Halite, Cu +1 brine, Sn 2+ It is one or more of the following: halide, phosphate, phosphite, formate, acetate, and oxalate.
[0065] In some preferred embodiments, the cocatalyst includes one or more of CuBr and Cu2PO3.
[0066] In some embodiments, the halide is a fluoride, chloride, bromide, or iodide. In some preferred embodiments, the halide is a chloride or bromide.
[0067] In some embodiments, the mass ratio of the co-catalyst to the Lewis acid is 0.1:100.0 to 1.0:100.0 or 0.1:100.0 to 0.8:100.0. In some embodiments, the mass ratio of the co-catalyst to the Lewis acid is 0.1:100.0, 0.2:100.0, 0.3:100.0, 0.4:100.0, 0.5:100.0, 0.6:100.0, 0.7:100.0 or 0.8:100.0.
[0068] In some embodiments, the reaction temperature of the complexation reaction is 10°C to 28°C.
[0069] In some embodiments, the reaction temperature of the Friedel-Crafts acylation reaction is -15°C to 5°C.
[0070] In some embodiments, the reaction temperature of the first reaction is 0°C to 25°C.
[0071] In some embodiments, the reaction time of the first reaction is 30 to 60 minutes.
[0072] In some embodiments, the reaction time of the first reaction is 4 to 6 hours.
[0073] In some embodiments, the post-processing includes: quenching the reaction with crushed ice, precipitating the polymer, allowing it to stand and separate into layers, removing the aqueous layer, washing the precipitate with water, evaporating the diluent, crushing the precipitate in an alcohol solution or water, filtering, washing with water, and drying to obtain the polyaryletherketone resin.
[0074] In some embodiments, the alcohol solution is an aqueous methanol solution with a concentration of 95% vol or higher, or an aqueous ethanol solution with a concentration of 95% vol or higher.
[0075] In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-1.25 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-1.00 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is 0.50 g / dl-0.91 g / dl. In some embodiments, the logarithmic viscosity of the aforementioned TS-PEKK resin is preferably 0.60 g / dl-0.88 g / dl.
[0076] Thirdly, the invention provides a use of the polyaryletherketone resin described in the first aspect or the polyaryletherketone resin obtained by the preparation method described in the second aspect.
[0077] The application of a polyaryletherketone resin as described in the first aspect or a polyaryletherketone resin obtained by the preparation method described in the second aspect in the preparation of polyaryletherketone resin-based prepregs or polyaryletherketone resin-based composites of fiber fabrics.
[0078] Fourthly, a polyaryletherketone resin-based prepreg for fiber fabrics is provided.
[0079] A polyaryletherketone resin-based prepreg for a fiber fabric, comprising: a fiber fabric and at least one polyaryletherketone resin selected from the polyaryletherketone resins described in the first aspect or the polyaryletherketone resins obtained by the preparation method described in the second aspect.
[0080] In some embodiments, the fiber fabric includes any one of carbon fiber, glass fiber, basalt fiber, boron nitride fiber, carbon nanotube fiber, graphene fiber, aramid fiber, polybenzoxazole (PBO), and polybenzimidazole (PBI).
[0081] In some embodiments, the fiber fabric shape is any one of plain weave fabric, twill weave fabric, satin weave fabric, three-dimensional woven fabric, or unidirectional fiber.
[0082] Fifthly, a polyaryletherketone resin-based composite material for fiber fabrics is provided.
[0083] A polyaryletherketone resin-based composite material for fiber fabrics is formed by melting and hot pressing the polyaryletherketone resin-based prepreg of the fiber fabrics described in the fourth aspect, followed by cooling and curing.
[0084] Beneficial effects
[0085] One embodiment provided by the present invention has at least one of the following beneficial effects:
[0086] (1) This invention uses self-made 1,3,5-triphenoxybenzene (TPOB) as the nucleating monomer B3. It has a symmetrical structure, stable properties, does not absorb water and deteriorate, and is easy to store. It can be co-condensed with aryl diacyl chloride A2 with B2 monomers such as DPODPS, DPE, 1,4- or 1,3-bis(4-phenoxybenzoyl)benzene (P-EKKE or m-EKKE), 1,4-diphenoxybenzene, 1,3-diphenoxybenzene, and 4,4'-diphenoxybenzophenone under Friedel-Crafts acylation reaction conditions to prepare thermoplastic resin varieties with different properties, such as soluble and molten star-shaped polyarylether ketone ketone (ST-PEKK) and star-shaped polyarylether ketone sulfone (ST-PEKKS).
[0087] (2) The molecular weight of the polymer, melt thermal oxidation stability and thermal properties of the resin are controlled by the molar mass and addition method of TPOB.
[0088] (3) The polyarylether ketone resin prepared is easy to separate and purify. The diluent DCM can be recycled and reused after distillation and azeotropic dehydration, which is conducive to energy conservation, emission reduction and environmental protection.
[0089] (4) The resin is pulverized in a wet state, which avoids the pollution of the production environment caused by resin dust in a dry state.
[0090] (5) The HCl gas released by the condensation reaction is absorbed by water and converted into dilute hydrochloric acid byproduct.
[0091] (6) The star-shaped PEAK and carbon fiber (CF) and other reinforcing materials prepared have good interfacial wettability. They can be made into carbon fiber composite prepregs by solvent method, slurry method, electrostatic powder impregnation method and melt impregnation method. High-strength and high-modulus composite materials are obtained by hot pressing. They have broad application prospects in aerospace, aviation, weapon equipment and civilian high technology fields.
[0092] (7) The polyaryletherketone resin provided by the present invention or the polyaryletherketone resin obtained by the provided preparation method has the advantages of high glass transition temperature, low melting temperature, good high and low temperature resistance, good solubility in common low toxicity organic solvents, and good melt thermal oxidation stability. Attached Figure Description
[0093] Figure 1 The image shows the secondary temperature rise curve of the ST-PEKKS-TM resin obtained in Example 1 using DSC (Differential Scanning Calorimetry).
[0094] Figure 2 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKKS-TM resin obtained in Example 1.
[0095] Figure 3 The image shows the TG-DTG (thermogravimetric analysis) curve of the ST-PEKKS-TM resin obtained in Example 1.
[0096] Figure 4 The image shows the secondary temperature rise curve of the ST-PEKKS-TS resin obtained in Example 9 using DSC (differential scanning calorimetry).
[0097] Figure 5 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKKS-TS resin obtained in Example 9.
[0098] Figure 6 The image shows the TG-DTG (thermogravimetric analysis) curve of the ST-PEKKS-TS resin obtained in Example 9.
[0099] Figure 7 The image shows the TG-DTG (thermogravimetric analysis) curve of the TS-PEKKS resin obtained in Example 18.
[0100] Figure 8 The image shows the secondary temperature rise curve of the TS-PEKKS resin obtained in Example 18 using DSC (differential scanning calorimetry).
[0101] Figure 9 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 39.
[0102] Figure 10 The image shows the TG (thermogravimetric analysis) curve of the ST-PEKK resin obtained in Example 39.
[0103] Figure 11 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 40.
[0104] Figure 12The image shows the TG (thermogravimetric analysis) curve of the ST-PEKK resin obtained in Example 40.
[0105] Figure 13 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 42.
[0106] Figure 14 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 43.
[0107] Figure 15 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 44.
[0108] Figure 16 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 45.
[0109] Figure 17 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 46.
[0110] Figure 18 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 47.
[0111] Figure 19 The image shows the DSC (Differential Scanning Calorimetry) curve of the ST-PEKK resin obtained in Example 48.
[0112] Terminology Definition
[0113] In the foregoing description of this invention, all figures disclosed herein, whether or not the words “approximately” or “about” are used, are approximate values. Based on the disclosed figures, the value of each figure may vary by less than ±10% or by a difference that is considered reasonable by those skilled in the art, such as ±1%, ±2%, ±3%, ±4%, or ±5%.
[0114] The terms "above", "below", and "within" are understood to include the number itself. For example, "two or more" means ≥ two.
[0115] The term “and / or” should be understood to mean any one of the options or any combination of two or more of the options.
[0116] The term "%vol" indicates a volume percentage.
[0117] "Prepreg" refers to a resin matrix and reinforcement composition that is made by impregnating continuous fibers or fabrics with a resin matrix under certain conditions, and can be stored.
[0118] The term "more" indicates a quantity of 2 or more, such as 2, 3, 4 or 5, etc.
[0119] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples. Detailed Implementation
[0120] To enable those skilled in the art to better understand the technical solutions of the present invention, some non-limiting embodiments are further disclosed below to provide a more detailed description of the present invention.
[0121] All reagents used in this invention can be purchased commercially or prepared by the methods described in this invention.
[0122] Logarithmic viscosity of resin (η) inh Determination: Prepare a 0.5 g / dL concentrated sulfuric acid solution of the resin and determine its concentration in a constant temperature water bath at 30℃±0.5℃, according to formula η. inh =C -1 ln(t1 / t0) is used for calculation; where C is the concentration of resin in concentrated sulfuric acid (g / dL), and t0 and t1 are the times the concentrated sulfuric acid solvent and the concentrated sulfuric acid resin solution flow through the capillary of the Ubbelohde viscometer, respectively, in seconds; Thermal oxidation stability test: referring to the method for evaluating the thermal oxidation stability of PEKK in WO840389, 2g of resin powder is placed on a stainless steel disc equipped with a high-temperature thermometer, heated to between 300 and 360℃ to melt, and samples are taken periodically in air to determine η. inh Change (△η) inh ) and observe the time (min) for the resin to maintain good flow.
[0123] Glass transition temperature (T) g ) or melting temperature (T) m Detection method: Differential scanning calorimetry (DSC) was used to determine the T of the polymer. g or T m The NETZSCHDSC214 differential scanning calorimeter was used, with a heating and cooling rate of 10 K / min and a test temperature range of 50–400 °C under a nitrogen atmosphere.
[0124] Thermal decomposition temperature (T) d Detection method: Thermogravimetric analysis (TGA) was performed using a NETZSCHTG 209F thermogravimetric analyzer to determine the thermal decomposition temperature (T) of the polymer. d The test temperature range is 20–800℃, and the heating rate is 20K / min.
[0125] Solubility test method:
[0126] Weigh 2g of dried resin and place it in a 25mL white volumetric flask. Add about 10mL of solvent and place it in a 30℃ constant temperature water bath for 3-6 hours, shaking the flask. Then add the same solvent to the mark, shake well, and let it stand. Observe the changes in the physical state of the resin.
[0127] a. Dissolved (+): The solute and solvent are homogeneous and transparent.
[0128] b. Swelling (+-): The solute and solvent are turbid and opaque, and swollen resin particles can be observed.
[0129] c. Insoluble (-): The solute and solvent are clearly separated into layers.
[0130] Main ingredients:
[0131] 1,3,5-Triphenoxybenzene (TPOB), self-prepared, MP: 112℃~113℃ (thermometer uncalibrated), structure determined by mass spectrometry and... 1 HNMR analysis and characterization;
[0132] 4,4′-Diphenoxydiphenyl sulfone (DPODPS), prepared in-house, MP: 139℃~141℃, structured by mass spectrometry. 1 HNMR characterization;
[0133] TPC, IPC, anhydrous AlCl3, DCM, DCE, etc. are all industrial products and are used directly without treatment. Industrial DPE is purified by vacuum distillation before use.
[0134] 1,4-Di(4-phenoxybenzoyl)benzene (p-EKKE), MP: 217℃; 1,3-Di(4-phenoxybenzoyl) (m-EKKE), MP: 122℃; were prepared according to “Synthesis and Characterization of 1,4-Di(4-phenoxybenzoyl)benzene” (Journal of Jiangxi Normal University (Natural Science Edition) 31(5) 519~522, 2007) and “Study on the Influence of Different Monomers on the Structure and Properties of Polyaryletherketone Ketone (PEKK)” (Acta Polymerica Sinica 2008, 10, 1016~1019).
[0135] In this invention, the abbreviations of compounds and their corresponding structures are as follows:
[0136]
[0137]
[0138] Examples 1-8 (Preparation of ST-PEKKS-TM), Control Example 1:
[0139] Monomers: TPOB (B3), DPODPS (B2), TPC (A2)
[0140] Operation Step A:
[0141] a) Mix AlCl3 (76g, 0.57mol) and co-catalyst CuBr (0.3g) with DCM (150ml), stir, cool to 0℃~5℃, add DMF (the amount of DMF added in each example and control example is shown in Table 1, where the molar amount of 15ml DMF is 0.205mol) and DCM (30ml), the complexation reaction is exothermic, the temperature rises to about 25℃, add DPODPS (the amount of DPODPS added in each example and control example is shown in Table 1), stir to dissolve, and obtain reaction mixture 1;
[0142] b) Cool the reaction mixture 1 to -10℃±5℃, add TPC (the amount of TPC added in each example and the control example is shown in Table 1), stir and react at -5℃±5℃ for 30 min to 60 min, add TPOB (the amount of TPOB added in each example and the control example is shown in Table 1), heat to 20℃±5℃ and continue stirring and reacting for 4 to 5 h.
[0143] c) Quench the reaction with 400 ml of ice water, stir to precipitate white granular resin, allow it to stand and separate into layers, wash the resin layer with deionized water, recover DCM by distillation, filter, crush the obtained resin multiple times in 95% ethanol, filter, wash with water, and dry to obtain ST-PEKKS resin (white fine granules). Analyze the logarithmic viscosity (η) of the obtained ST-PEKKS resin. inh Glass transition temperature (T) g ), melting temperature (T) m ), thermal decomposition temperature (T) d The results for the solubility are shown in Table 1.
[0144] The structural formula of ST-PEKKS-TM:
[0145]
[0146] Table 1: Preparation and Thermal Performance Test Results of ST-PEKKS-TM
[0147]
[0148] Note: Tg is the value of the second temperature rise curve of DSC. Tg has the same meaning in the following text.
[0149] In the solubility section, "-" indicates insolubility; "+-" indicates swelling; and "+" indicates solubility. The symbols in the following text have the same meaning.
[0150] Conclusion: The Tg of the copolymer increases by more than 4°C and the Tm decreases by 15°C, which is beneficial for reducing the melt processing temperature of the resin.
[0151] Examples 9-12 (Preparation of ST-PEKKS-TS resin), Comparative Example 2:
[0152] In the preparation methods of Examples 1-8, the A2 monomer TPC was replaced with TPC and / or IPC. The types of other monomers and reagents were the same as in Examples 1-8. Each monomer and Lewis base was added according to the amounts shown in Table 2. The preparation was carried out according to the methods of Examples 1-8 to obtain ST-PEKKS-TS resin. The logarithmic viscosity (η) of the obtained ST-PEKKS-TS resin was measured. inh Glass transition temperature (T) g ), melting temperature (T) m ), thermal decomposition temperature (T) d The results for the solubility are shown in Table 2.
[0153] Table 2: Preparation and Thermal Performance Test Results of ST-PEKKS-TS
[0154]
[0155] in conclusion:
[0156] In Table 2, "*" indicates that no crystallization melting peak was observed on the second heating curve of DSC.
[0157] Compared to Example 12, the Tg of Example 11 increased by 10°C while the Tm remained close; compared to Control Example 2, the Tg of Example 11 was 9°C higher. Experiments show that when DPODPS is copolymerized with TPC / IPC and the molar ratio of TPC to IPC is less than 0.60:0.40, the polymer transforms into an amorphous structure.
[0158] ST-PEKKS-TS has a slightly crystalline aggregated state, which is conducive to its dissolution in solvents such as DMF, NMP or halogenated hydrocarbons, and facilitates its use in wet processes to combine with reinforcing materials to produce composite prepregs.
[0159] Examples 13-31: Preparation of TS-PEKKS Resin
[0160] Preparation method: The monomer molar mass ratios in Examples 13-31 are the same as in Example 9. Refer to step A to prepare ST-PEKKS-TS copolymers with different ηinh. Thermal oxidative stability test: Take the TS-PEKKS resins obtained in Examples 13-18 and test the initial ηinh. inh The values were determined by placing the samples at 330℃±10℃ for 0.5h, 1h, 2h, and 3h, respectively, and measuring η at different time points. inh The values are shown in Table 3.
[0161] Melt flow index: Examples 19-24 were tested using a melt flow rate tester according to the national standard method (GB3682-2000), and the results are listed in Table 4.
[0162] Mechanical properties of TS-PEKKS-TS / CF (fabric) composite laminates: Prepregs were prepared by combining two commercially available carbon fiber fabrics with the TS-PEKKS-TS resin obtained in Examples 25-31 (Examples 25-31 used soluble TS-PEKKS with different nh values, and the monomer molar ratio was the same as in Example 9). The prepregs were then hot-pressed under programmed temperature to form laminates, resulting in TS-PEKKS-TS / CF (fabric) composite laminates. Standard specimens were cut and their mechanical properties were tested according to GB-T1447-2005. The test results of the mechanical properties of the TS-PEKKS-TS / CF (fabric) composite laminates are listed in Table 5.
[0163] Table 3: Thermal and Oxidative Stability of TS-PEKKS Resin
[0164]
[0165] Table 4: Melt Flow Index of TS-PEKKS Resin*
[0166]
[0167] *Instrument Name: Melt Flow Rate Tester
[0168] Conclusion: As shown in Tables 3 and 4, the TS-PEKKS resin provided by this invention exhibits excellent thermal oxidation stability, melt flowability, and molecular weight (η). inh The η value is inversely proportional to the η value of TS-PEKKS resin, the matrix resin for carbon fiber (CF) composites. inh The preferred value is 0.65±0.05 g / dl.
[0169] Table 5: Mechanical Properties of TS-PEKKS-TS / CF (Fabric) Composite Laminates
[0170]
[0171]
[0172] Conclusion: The soluble TS-PEKKS resin prepared in this invention exhibits a high glass transition temperature (Tg) and a low melt transition temperature (Tm), low melt viscosity, and good thermal stability. It also demonstrates excellent wettability with carbon fibers T3003K (fabric) and T70012K (fabric). Through wet impregnation, it can be formulated into prepregs, and after hot pressing, it can be used to produce high-strength, high-modulus ST-PEKKS / CF (fabric) composite structural components. It has broad application prospects in aerospace, military equipment, and high-end civilian fields.
[0173] Examples 32-38: Preparation of ST-PEKKS-TH resin (TH indicates high temperature resistant type)
[0174] Monomers: B3: TPOB, B2: DPODPS, DPE or p-EKKE, A2: TPC
[0175] Implementation Step B:
[0176] AlCl3 (72-85g) was mixed with DCM (150ml-180ml), and DCM mixture containing DMF (or NMP) (Lewis base, see Table 6 for dosage) was added. The temperature was controlled below 25°C. Then, DPODPS and p-EKKE from monomer B2 were added, where p-EKKE and DPODPS formed a complex with aluminum trichloride. The mixture was stirred until DPODPS and p-EKKE were completely dissolved and became transparent. The mixture was cooled to -10°C ± 5°C, monomer A2 was added, and the mixture was reacted at -5°C to 5°C for 30min to 1h. Monomer B3 was added, and the mixture was reacted at 5°C to 10°C for 1h to 2h, at 15°C ± 5°C for 2h, and then at 20°C ± 5°C for 1h. The resins prepared in Comparative Examples 3, 32, 33, and 34 also included the addition of DPE and a reaction time of 1h. The reaction was quenched with cold water, methanol, or a 95% ethanol aqueous solution. After solid-liquid separation, the resin was repeatedly crushed in 95% ethanol, washed with water, and dried to obtain ST-PEKKS-TH resin. The logarithmic specific viscosity (η) of the obtained ST-PEKKS-TH resin was measured. inh Glass transition temperature (T) g ), melting temperature (T) m ) and thermal decomposition temperature (T d The results are shown in Table 6.
[0177] Table 6: Preparation of ST-PEKKS-TH
[0178]
[0179]
[0180] In Table 6, "*" indicates that as the molar content of diphenoxydiphenyl sulfone structural units (DPODPS) in the terpolymer molecular chain increases (e.g., the ratio in Examples 35 and 36), the glass transition temperature (Tg) increases and the crystallization melting temperature (Tm) decreases. However, when the molar content of diphenoxydiphenyl sulfone structural units (DPODPS) is high enough (e.g., the ratio in Example 38), it is difficult to detect the crystallization melting peak (Tm) on the DSC heating curve.
[0181] Conclusion: Examples 32-38 are terpolymers containing star-shaped structural units. Compared with PEKK (Tg: 156℃, Tm: 356℃), ST-PEKKS-TH has a higher Tg. g There has been a significant increase, T m T d It is comparable to PEKK.
[0182] Examples 39-48: Preparation of ST-PEKK Resin
[0183] Monomers: B3: TPOB; B2: at least one of DPE, p-EKKE, m-EKKE, etc.; A2: TPC and / or IPC.
[0184] Implementation Step C:
[0185] a. Mix anhydrous aluminum trichloride (calculation of the amount of anhydrous aluminum trichloride: ① Amount of anhydrous aluminum trichloride for complexation reaction: the amount of anhydrous aluminum trichloride required to form a complex with carbonyl groups, amide groups, etc. in the reaction system in a molar ratio of 1.0:1.0 + ② Amount of anhydrous aluminum trichloride for acylation reaction: 0.5 to 1.2 times the molar amount of aromatic diacyl chloride added) and co-catalyst CuBr (0.3 g) with DCM (150 to 180 ml), and add a mixture of Lewis base DMF, DMAc or NMP and diluent DCM at 10℃±5℃. The molar amount of the Lewis base added is... The amount of aluminum trichloride added is 0.2 times the molar amount of aramid chloride, followed by monomer B2 (DPE, p-EKKE, and / or m-EKKE, see Table 7 for types and amounts). Aluminum trichloride reacts with monomer B2 to form a complex. The mixture is stirred to obtain reaction mixture 1. Reaction mixture 1 is cooled to -15℃±5℃, monomer A2 (TPC and / or IPC, see Table 7 for types and amounts) is added, and the reaction is carried out for 30 min to 1 h. The temperature is then raised to 5℃ to 15℃, and monomer B3 TPOB (see Table 7 for amounts) is added. The polycondensation reaction is continued at 15℃ to 25℃ for 5 to 6 h. The molar concentration of the monomers is controlled at 0.2-0.6 mol / L (the molar concentration of the monomers refers to the molar concentration of all monomers (A2+B2+B3) in diluted DCM with Lewis base, which can be adjusted accordingly based on the implementation of the polycondensation reaction).
[0186] b. Quenching reaction
[0187] After the polycondensation reaction was completed, 300-500 ml of ice water was added to decompose the complex formed by ST-PEKK and AlCl3, and the mixture was stirred to obtain a white, fine granular resin. The DCM was evaporated by heating to 50℃±5℃, and the solid-liquid mixture was separated to obtain ST-PEKK resin (white). The ST-PEKK resin was repeatedly crushed in 95% ethanol or methanol, and then washed with water until no chloride ions were detected in the washing liquid using silver nitrate ammonia solution. The resin was then dried to obtain purified ST-PEKK resin. The melt thermal stability of the ST-PEKK resins obtained in Examples 47 and 48 at 360℃-380℃ was tested, and the results are shown in Table 8.
[0188] Table 7: Preparation and Thermal Properties of ST-PEKK
[0189]
[0190] In Table 7, "*" indicates powder samples.
[0191] In Table 7, "**" indicates the sample after melting.
[0192] The thermal properties of ST-PEKK are closely related to its thermal history. Samples 45* and 46* are unmelted ST-PEKK powders.
[0193] The second DSC heating curve showed that the Tg of 45* was 163.9–165.3℃ and the Tm was 362.8℃, while the Tg of 46* was 154.1–169.7℃. Cold crystallization peaks (Tc) appeared at 294.8℃ and 297.6℃ on the DSC cooling curve. The remaining samples, including 42**, were molten samples, and showed a melting exothermic peak at around 200℃ on the DSC heating curve, followed by a crystallization melting peak.
[0194] Conclusion: PEKK resins prepared using hydrophilic monomers such as DPE, TPC, and IPC are employed. The biggest problem with PEKK preparation using DPE as the aromatic ether monomer is the insufficient melt thermal stability of the resin. The thermal properties (Tg, Tm, Td) of PEKK are closely related to the molar ratio of para- and meta-phenyl groups in the molecular chain. A higher molar ratio of para-phenyl groups increases Tg and Tm, but the melt processing temperature also increases accordingly, limiting its practical application range. The molar ratio of para- and meta-phenyl groups in PEKK resins with practical application value is generally controlled by the molar ratio of TPC / IPC. The para- and meta-phenyl group molar ratio of commercially valuable PEKK is generally 70–30 / 30–70.
[0195] This invention prepares ST-PEKK resin using p-EKKE and m-EKKE as B2 monomers, TPOB as B3 monomer, and TPC and IPC as A2 monomers. The molar ratio of para- and meta-phenyl groups in the ST-PEKK macromolecule is controlled by simultaneously adjusting the molar ratio of B2 and A2 monomers, thereby obtaining ST-PEKK resin with the desired thermal properties and molecular weight. Comparing the experimental results of Examples 39 and 40, the prepared ST-PEKK resins all have a para- and meta-phenyl group molar ratio of 5 / 5, and their Tg, Tm, and Td are also relatively close. It is generally believed that the η of PEKK resin... inh Resins with a concentration greater than 0.60 g / dl are classified as high molecular weight resins. inh An increase in the value of η leads to higher melt viscosity and deterioration of melt processing performance, therefore η inh Generally controlled at 0.62–0.85 g / dl, η inh PEKK with a value of 0.65–0.75 g / dl has a low melt viscosity and is suitable as a matrix resin for high-performance composite materials.
[0196] As a high-performance thermoplastic polymer material, ST-PEKK resin requires that the resin be as stable as possible at the melt processing temperature, and should not have obvious oxidative crosslinking and degradation. Table 8 lists the melt thermal oxidation stability test results of PEKK and ST-PEKK resins prepared in Examples 48 and 47 at 360-380°C. As can be seen from Table 8, the melt thermal oxidation stability of ST-PEKK in Example 47 is better than that in Example 48.
[0197] Table 8: Melt thermal stability of ST-PEKK resin and PEKK resin at 360–380℃
[0198]
[0199] Table 9: Melt Flow Index (MFR) of PEKK and ST-PEKK Resins*
[0200]
[0201] Melt index measurements showed (see Table 9) that Example 47 had better melt flowability than Example 48.
[0202] Example 49: Mechanical property testing of ST-PEKK / CF composite laminate
[0203] Prepregs were prepared by combining two commercially available carbon fiber fabrics (T700-3K and T800-6K) with the ST-PEKK resin obtained in Example 39. Powdered resin was uniformly coated onto the surface of the CF (fiberglass) fabric at a resin content of 42% ± 3%. The lamination pressure was 12 MPa, and the temperature was 360℃~380℃ to obtain ST-PEKK / CF composite laminates. These were cut into standard specimens, and their mechanical properties were tested according to GB / T1447-2005 and GB / T 9341-2008 methods. The average value of five specimens was taken. The mechanical property test results of the ST-PEKK / CF composite laminates are listed in Table 10.
[0204] Table 10: Mechanical property testing of ST-PEKK / CF composite laminate
[0205] ST-PEKK / T700-3K ST-PEKK / T800-6K Test Standards Tensile strength / MPa 754 847 GB / T1447-2005 Tensile modulus / GPa 56.4 58 GB / T1447-2005 Bending strength / MPa 837 975 GB / T9341-2008 Flexural modulus / GPa 67.2 75.3 GB / T9341-2008
[0206] Conclusion: The soluble ST-PEKK resin prepared in this invention exhibits a high glass transition temperature (Tg) and a low melt transition temperature (Tm), low melt viscosity, good thermal stability, and excellent wettability with carbon fibers (such as T700-3K and T800-6K). It can be wet-impregnated to produce prepregs, and hot-pressed to create high-strength, high-modulus ST-PEKK / CF composite structural components. It has broad application prospects in aerospace, military equipment, and high-end civilian fields.
[0207] The method of this invention has been described through preferred embodiments. Those skilled in the art will readily be able to modify or appropriately alter and combine the methods and applications described herein within the scope, spirit, and context of this invention to implement and apply the technology of this invention. Those skilled in the art can refer to the content herein to appropriately improve process parameters. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included within the scope of this invention.
Claims
1. A polyaryletherketone resin with the structure shown in Formula I, (I); in, A2 has an aramid structure; B2 has an aromatic ether structure; B3 is selected from: ; m, n, and p represent the degree of polymerization; The aramid structure is as follows: and ; The aromatic ether structure is as follows: , , , One or more of the following; The and The molar ratio is (9~1):(1~9); The logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl - 1.25 g / dl.
2. The polyaryletherketone resin according to claim 1, wherein the logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl-1.20 g / dl.
3. The polyaryletherketone resin according to claim 1, wherein the logarithmic viscosity of the polyaryletherketone resin is 0.60 g / dl-0.86 g / dl.
4. A method for preparing the polyaryletherketone resin according to any one of claims 1-3, comprising: reacting mesityleneoxybenzene, aryl ether, and aryl diacyl chloride in a catalyst solvent system, followed by post-treatment to obtain the polyaryletherketone resin; or It includes: The aromatic ether is mixed with a catalyst solvent system to undergo a complexation reaction, followed by the addition of aryl diacyl chloride for Friedel-Crafts acylation, and then the addition of mestriphenoxybenzene for the first reaction. After post-treatment, the polyaryl ether ketone resin is obtained. The aramid chloride is and ; The aromatic ether is: , , , One or more of them.
5. The preparation method according to claim 4, wherein the logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl - 1.00 g / dl; and / or The molar ratio of the triphenoxybenzene (B3) to the aryl ether (B2) is (0.3~1.5):100.0; and / or The molar ratio of the aromatic ether (B2) to the aryl dichloroisocyanurate (A2) is (1.00~1.05):1.00; and / or The catalyst solvent system includes a diluent, a Lewis acid, a Lewis base, and a co-catalyst.
6. The preparation method according to claim 5, The diluent includes an aprotic organic solvent; the aprotic organic solvent includes one or more of dichloromethane (DCM), dichloroethane (DCE), chloroform, o-dichlorobenzene, and tetrachloroethane; and / or Each 1L of the diluent contains 0.10mol to 0.80mol of arethanediol chloride; and / or The Lewis acid includes one or more of AlCl3, FeCl3, and InCl3; and / or The molar amount of the Lewis acid feed is the total molar amount of ketone, amide, and sulfone groups in the feed for the complexation reaction, plus the molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction. The molar amount of the Lewis acid required for catalysis in the Friedel-Crafts acylation reaction is 0.5 to 2.2 times the molar amount of the aramid chloride feed; and / or The Lewis base includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), sulfolane, and diphenyl sulfone; and / or The molar ratio of the Lewis base to the aramid chloride is (0.2~2.0):1.0; and / or The co-catalyst comprises organic acid salts or inorganic acid salts; and / or The mass ratio of the co-catalyst to the Lewis acid is (0.1~0.8):100.
0.
7. The preparation method according to any one of claims 4-5, The reaction temperature for the complexation reaction is 10℃~28℃; and / or The Friedel-Crafts acylation reaction is performed at a temperature of -15°C ± 5°C, and / or; The reaction temperature of the first reaction is 0℃~25℃; and / or The post-processing includes: The reaction is quenched by adding ice, and a precipitate is obtained. After standing and separating into layers, the aqueous layer is removed, the precipitate is washed with water, the diluent is evaporated, the precipitate is crushed in an alcohol solution or water, filtered, washed with water, and dried to obtain the polyaryletherketone resin.
8. The preparation method according to claim 5, The logarithmic viscosity of the polyaryletherketone resin is 0.50 g / dl - 0.91 g / dl; and / or The cocatalyst includes Fe 2+ Halite, Cu +1 brine, Sn 2+ One or more of the following: halide, phosphate, phosphite, formate, acetate, and oxalate; and / or The mass ratio of the co-catalyst to the Lewis acid is (0.1~0.8):100.
0.
9. The preparation method according to claim 6, The aprotic organic solvent includes one or more of dichloromethane, dichloroethane, and o-dichlorobenzene; and / or Each 1L of the diluent contains 0.30mol to 0.70mol of arethanediol chloride; and / or The Lewis acid is AlCl3.
10. The preparation method according to claim 8, The logarithmic viscosity of the polyaryletherketone resin is 0.60 g / dl - 0.86 g / dl; and / or The co-catalyst includes one or more of CuBr, CuCl, and Cu2PO3.
11. The use of a polyaryletherketone resin according to any one of claims 1-3 or a polyaryletherketone resin obtained by the preparation method according to any one of claims 4-10 in the preparation of polyaryletherketone resin-based prepregs for fiber fabrics or polyaryletherketone resin-based composites for fiber fabrics.
12. A polyaryletherketone resin-based prepreg for fiber fabrics, comprising: The fibrous fabric and at least one polyaryletherketone resin selected from the polyaryletherketone resins according to any one of claims 1-3 or the polyaryletherketone resins obtained by the preparation method according to any one of claims 4-10.
13. The polyaryletherketone resin-based prepreg for fiber fabrics according to claim 12, wherein the fiber fabric comprises any one of carbon fiber, glass fiber, basalt fiber, boron nitride fiber, carbon nanotube fiber, graphene fiber, aramid fiber, polybenzoxazole or polybenzimidazole.
14. The polyaryletherketone resin-based prepreg of the fiber fabric according to any one of claims 12-13, wherein the fiber fabric is any one of plain weave, twill weave, satin weave, three-dimensional woven fabric, or unidirectional fiber.
15. A polyaryletherketone resin-based composite material for fiber fabrics, which is formed by melting and hot pressing the polyaryletherketone resin-based prepreg of the fiber fabrics according to any one of claims 12-14, followed by cooling and curing.
Citation Information
Patent Citations
Method for preparing high molecular weight polyaryletherketone
CN107987272A
Functionalized polymer particles for use as toughening agent
CN106459560A
Polyaryl-ether-ketone viscosity regulator synthesized based on A2+B3 type monomer reaction and method therefor
CN1640912A