Granular carbon black and preparation method thereof, electrode and secondary battery

By regulating the particle size distribution and secondary particle size of granular carbon black, and using the wet granulation process with water as the only additive, the problems of low strength, severe pulverization and poor dispersion in the carbon black granulation process are solved, achieving high The bulk density and good dispersion improve their application performance in batteries and other fields.

CN117757288BActive Publication Date: 2024-11-19JIAOZUO CITY HEXING CHEMICAL INDUSTRY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311791345.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-11-19
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

The existing carbon black granulation process leads to low strength, serious pulverization of granular carbon black, and insufficient bulk density and dispersion, which affects its application performance in batteries and other fields.

Method used

By coordinating the secondary particle size D50 and particle size distribution range of granular carbon black, wet granulation process with water as the only additive, combined with the regulation of stirring speed and time, we ensure that the particle size distribution of granular carbon black is particle size < The proportion of 0.125mm is ≤2wt%, the proportion of 0.125-0.85mm is 18wt%~60wt%, and the proportion of >0.85mm is 40wt%~80wt%, and the secondary particle size D50 is controlled to be 2.0-3.51μm, and the particles are Strength ≤5.3gf/piece.

Benefits of technology

It significantly improves the bulk density and dispersion of granular carbon black, reduces the pulverization phenomenon, and ensures its uniform distribution and performance in the electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117757288B_ABST
    Figure CN117757288B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of carbon black materials, and in particular to a granular carbon black and a preparation method thereof, an electrode and a secondary battery. Granular carbon black, the particle size distribution range of the granular carbon black is as follows: the proportion of granular components with a particle size of less than 0.125 mm is ≤2wt%, the proportion of granular components with a particle size of 0.125 to 0.85 mm is 18wt% to 60wt%, and the proportion of granular components with a particle size of more than 0.85 mm is 40wt% to 80wt%; the secondary particle size D50 of the granular carbon black is 2.0 to 3.51μm. The granular carbon black of the present invention has a suitable particle size distribution, which not only reduces the pulverization phenomenon, but also can significantly improve the bulk density and dispersibility, and helps to give full play to the conductive properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon black materials, and in particular to granular carbon black and a preparation method thereof, an electrode and a secondary battery. Background Art

[0002] Most process applications involving carbon black require it to be granulated. Traditionally, the granulation process includes adding water or a binder to the carbon black powder for granulation and drying. At present, the existing carbon black granulation process only adds water to granulate the carbon black powder, and the strength of the obtained granular carbon black is relatively low, which will lead to pulverization during subsequent transportation or use. At the same time, the existing carbon black granulation process, in the granulation process of adding only water, has poor stirring uniformity, which will cause large fluctuations in the particle size after granulation, and the bulk density is limited compared to the carbon black powder.

[0003] In addition, although the use of additives to granulate carbon black powder can improve the strength of the particles, it will introduce impurities and cause poor dispersion due to segregation of agglomerated particles.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide granular carbon black and a preparation method thereof, an electrode and a secondary battery, so as to solve the technical problems existing in the prior art such as pulverization of granular carbon black, low bulk density and poor dispersibility.

[0006] In order to achieve the above-mentioned object of the present invention, the present invention provides granular carbon black on one hand, and the particle size distribution range of the granular carbon black is as follows:

[0007] The proportion of granular components with a particle size of less than 0.125 mm is ≤ 2wt%, the proportion of granular components with a particle size of 0.125 to 0.85 mm is 18wt% to 60wt%, and the proportion of granular components with a particle size of more than 0.85 mm is 40wt% to 80wt%;

[0008] The secondary particle size D50 of the granular carbon black is 2.0 to 3.51 μm.

[0009] In a specific embodiment of the present invention, the apparent specific volume of the granular carbon black is 3.2 to 3.4 mL / g.

[0010] In a specific embodiment of the present invention, the DBP oil absorption value of the granular carbon black is X1, the DBP oil absorption value of the powdered carbon black obtained by granulating the granular carbon black is X2, and X1 and X2 satisfy: (X2-X1) / X2 is 14.3% to 26.5%.

[0011] In a specific embodiment of the present invention, the secondary particle size D50 of the granular carbon black is Y1, the secondary particle size D50 of the powdered carbon black obtained by granulation is Y2, and Y1 and Y2 satisfy: (Y2-Y1) / Y2 is 60.2% to 77.3%.

[0012] In a specific embodiment of the present invention, the particle strength of the granular carbon black is ≤5.3 gf / piece, such as 4.6 to 5.3 gf / piece.

[0013] In a specific embodiment of the present invention, the raw material of the granular carbon black is acetylene black.

[0014] Another aspect of the present invention provides a method for preparing any one of the above-mentioned granular carbon blacks, comprising the following steps: wetting the powdered carbon black with water, and then wet granulating and drying;

[0015] In the wet granulation, the stirring speed is firstly 2200-2800 r / min for 15-25 min, and then the stirring speed is 1200-1800 r / min for 2-8 min.

[0016] The mass ratio of the powdered carbon black to the water is 1:(2-2.5).

[0017] In a specific embodiment of the present invention, during the wetting, a pre-stirring process is performed at a stirring speed of 1000 to 1400 r / min. Furthermore, the pre-stirring process lasts for 1 to 5 minutes.

[0018] In a specific embodiment of the present invention, the temperature of the water is ≥ 60°C.

[0019] In a specific embodiment of the present invention, the powdered carbon black is acetylene carbon black.

[0020] Another aspect of the present invention provides an electrode, comprising any one of the above-mentioned granular carbon blacks.

[0021] Another aspect of the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator; at least one of the positive electrode and the negative electrode is any one of the electrodes described above.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The granular carbon black of the present invention has a suitable particle size distribution, which not only reduces the pulverization phenomenon, but also can significantly improve the bulk density and dispersibility;

[0024] (2) The preparation method of the granular carbon black of the present invention is simple to operate, does not introduce additional additives, does not cause particle segregation and pollution, and further ensures the dispersibility of the granular carbon black. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 A schematic diagram of the structure of an apparatus for preparing granular carbon black provided in an embodiment of the present invention.

[0027] Reference numerals:

[0028] 1- Granulation barrel; 2- Mixing paddle. DETAILED DESCRIPTION

[0029] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] Carbon black has excellent electrical conductivity and is widely used in batteries, resins, rubber and other fields. The carbon black initially produced is in powder form. Due to its low bulk density and easy pulverization, the powdered carbon black is usually granulated to improve its usability and transportation convenience.

[0031] With the development requirements of related fields, it is necessary not only to reduce the pulverization problem of granular carbon black obtained by granulation, but also to increase the packing density of granular carbon black so that it can be easily dispersed evenly in the matrix in downstream applications to ensure full performance.

[0032] However, currently, powdered carbon black is granulated by adding water. Since no other binders are added and carbon black has a developed structure, the particle strength of the granulated carbon black after granulation is lower than that of general conductive granular carbon black. Therefore, when it is mixed with resin and / or rubber or transported, it will be pulverized, affecting its use. At the same time, the granular carbon black obtained by granulation by adding only water has a large fluctuation in the particle range, and the improvement of the bulk density is limited. The number of particles contained in a certain mass of carbon black is relatively small, and it is not easy to be evenly distributed in the resin, rubber or electrode material in downstream applications, and the dispersion is poor. When powdered carbon black is granulated with additives such as binders, although the particle strength can be improved, impurities will be introduced and affect its use.

[0033] The inventor has found through research that during the production of carbon black, the primary particles will melt into larger three-dimensional and chain-branched structure aggregates, which are called carbon black primary structures. The secondary particle size is a measure of the particle diameter of the primary structure. The more developed the aggregate branches are, the larger the internal voids are, and the higher the carbon black primary structure is. This aggregate with developed branched chains and void structures is further agglomerated into agglomerates and carbon black particles through physical effects such as van der Waals forces. During the use of carbon black, the agglomerates of carbon black are opened into primary structures through sanding, grinding, etc., which improves the dispersion of carbon black in electrode materials, rubber, or plastics, and improves the application effect of carbon black. As the secondary particle size decreases, carbon black can be better dispersed during the application process, improving dispersibility. The reduction in secondary particle size guarantees dispersibility to a certain extent, but the improvement in bulk density is insufficient, resulting in an insufficient number of particles in a certain volume of granular carbon black.

[0034] When the granular carbon black has a suitable particle size distribution, the particles with relatively small particle size can fully fill the vacancies between the particles with relatively large particle size to increase the packing density. If the particle size is too small, it will not only fail to fill effectively but also cause pulverization; and if there are too few particles with relatively low particle size, there will be fewer vacancies and it will not be able to fill effectively; and too many small particles will introduce the risk of aggregation and insufficient dispersion.

[0035] The present invention coordinately regulates the secondary particle size D50 of the granular carbon black and the particle size distribution range of the granular carbon black, thereby ensuring both the dispersibility and the bulk density of the granular carbon black and reducing the pulverization phenomenon.

[0036] Based on this, the present invention provides granular carbon black on one hand, and the particle size distribution range of the granular carbon black is as follows:

[0037] The proportion of granular components with a particle size of less than 0.125 mm is ≤ 2wt%, the proportion of granular components with a particle size of 0.125 to 0.85 mm is 18wt% to 60wt%, and the proportion of granular components with a particle size of more than 0.85 mm is 40wt% to 80wt%;

[0038] The secondary particle size D50 of the granular carbon black is 2.0 to 3.51 μm.

[0039] Among them, the proportion of granular components with a particle size of less than 0.125mm may be 2wt%, 1.8wt%, 1.5wt%, 1.2wt%, 1wt%, 0.8wt%, 0.5wt%, 0.2wt% or a range consisting of any two of them; the proportion of granular components with a particle size of 0.125-0.85mm may be 18wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt% or a range consisting of any two of them; the proportion of granular components with a particle size of more than 0.85mm may be 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt% or a range consisting of any two of them.

[0040] Granular components with a particle size range of 0.125 to 0.85 mm can effectively fill the vacancies formed by granular components with a particle size greater than 0.85 mm, greatly improving the packing density, so that a certain volume of granular carbon black has as many particles as possible, and can be more easily and evenly distributed in electrode materials, resins and / or rubbers during the application process, thereby improving dispersibility and preventing pulverization problems.

[0041] In a specific embodiment of the present invention, the apparent specific volume of the granular carbon black is 3.2 to 3.4 mL / g.

[0042] The apparent specific volume of carbon black is determined by referring to the method of GB / T 3781.6. The apparent specific volume of the granular carbon black of the present invention can be 3.2 mL / g, 3.25 mL / g, 3.3 mL / g, 3.35 mL / g, 3.4 mL / g or a range consisting of any two of them. When the particle size distribution of the granular carbon black of the present invention meets the above conditions, the bulk density can be effectively improved, and the corresponding apparent specific volume of the granular carbon black is within the above range.

[0043] In a specific embodiment of the present invention, the DBP oil absorption value of granular carbon black is X1, and the DBP oil absorption value of powdered carbon black obtained by granulation is X2, and X1 and X2 satisfy: (X2-X1) / X2 is 14.3% to 26.5%.

[0044] Among them, the DBP oil absorption values ​​of granular carbon black and powdered carbon black are tested with reference to the method of GB / T 14853.6.

[0045] For example, in different embodiments, the rate of change (X2-X1) / X2 of the DBP oil absorption value of the powdered carbon black for preparing granular carbon black before and after granulation can be 14.3%, 15%, 16.3%, 18.4%, 20%, 22%, 22.4%, 24.6%, 25%, 26.5% or a range consisting of any two of them.

[0046] In a specific embodiment of the present invention, the secondary particle size D50 of granular carbon black is Y1, the secondary particle size D50 of powdered carbon black obtained by granulation is Y2, and Y1 and Y2 satisfy: (Y2-Y1) / Y2 is 60.2% to 77.3%.

[0047] For example, in different embodiments, the change rate (Y2-Y1) / Y2 of the secondary particle size D50 of the powdered carbon black for preparing granular carbon black before and after granulation can be 60.2%, 62%, 63.7%, 64.9%, 65%, 68%, 70%, 72%, 75%, 77.1%, 77.3% or a range composed of any two of them.

[0048] The overall structure of carbon black is a measure of the complexity of carbon black aggregate particles, which is often expressed as an oil absorption value, specifically referring to the number of milliliters of adsorbed oil relative to 100g of carbon black. When carbon black has a relatively high DBP oil absorption value, it indicates that the carbon black has a relatively high structure or volume occupancy property. The DBP oil absorption value of carbon black is determined by referring to the method of GB / T 14853.6. In the present invention, the secondary particle size D50 of granular carbon black is significantly reduced compared with that of powdered carbon black to meet the requirements of dispersibility; at the same time, the appearance and structure of the granular carbon black obtained by granulation are changed compared with those of powdered carbon black, and the change rate of the DBP oil absorption value before and after granulation can be maintained within the corresponding range, indicating that the microscopic porous structure in the granular carbon black is still retained to a large extent, greatly reducing the impact on the performance of the granular carbon black.

[0049] In a specific embodiment of the present invention, the particle strength of the granular carbon black is ≤5.3 gf / piece, such as 4.6 to 5.3 gf / piece.

[0050] The particle strength of granular carbon black is measured with reference to the method of GB / T 14853.6. For example, in different embodiments, the particle strength of the granular carbon black of the present invention can be 4.6gf / piece, 4.7gf / piece, 4.8gf / piece, 4.9gf / piece, 5gf / piece, 5.1gf / piece, 5.2gf / piece, 5.3gf / piece, or a range consisting of any two of them. When the particle strength is within the above range, it can be ensured that it is not easy to break during transportation, and at the same time, it can be ensured that it has a high crushing rate when mixed with other materials in the subsequent use, thereby improving the dispersibility.

[0051] In a specific embodiment of the present invention, the raw material powder carbon black of the granular carbon black is selected from any one of acetylene carbon black, furnace black, channel black, lamp black and thermal black. It is understood that in a specific embodiment of the present invention, acetylene carbon black is used as the powder carbon black to exemplify the granular carbon black and its preparation method, but it does not limit the type of the powder carbon black of the present invention.

[0052] Another aspect of the present invention provides a method for preparing any one of the above-mentioned granular carbon blacks, comprising the following steps: wetting the powdered carbon black with water, and then wet granulating and drying;

[0053] In the wet granulation, the stirring speed is firstly 2200-2800 r / min for 15-25 min, and then 1200-1800 r / min for 2-8 min.

[0054] The mass ratio of powdered carbon black to water is 1:(2-2.5).

[0055] In wet granulation, high-speed shearing is first used to depolymerize the carbon black structure and reduce the secondary particle size of carbon black. Within the stirring treatment time range of 15 to 25 minutes, the secondary particle size continues to decrease; when the corresponding stirring time is exceeded, the particles produce complex agglomeration, causing the macroscopic particle size of the granular carbon black to increase. After this stage, the particle size distribution range of the granular carbon black is adjusted by adjusting the stirring speed. When the rotation speed increases, the particle size range changes to a small size, when the rotation speed is slow, the particle size range changes to a large size, and when the time is extended, the particle size range changes to a large size. By adjusting the rotation speed and time within the above range, granular carbon black with a secondary particle size D50 and a particle size distribution that meet the requirements can be obtained.

[0056] For example, in different embodiments, in the wet granulation, the stirring speed can be first 2200 r / min, 2400 r / min, 2500 r / min, 2600 r / min, 2800 r / min or any range consisting of two thereof for stirring for 15 min, 18 min, 20 min, 22 min, 25 min or any range consisting of two thereof; and then the stirring speed can be 1200 r / min, 1400 r / min, 1500 r / min, 1600 r / min, 1800 r / min or any range consisting of two thereof for stirring for 2 min, 4 min, 5 min, 6 min, 8 min or any range consisting of two thereof.

[0057] The mass ratio of powdered carbon black to water can be 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5 or a range consisting of any two of them.

[0058] The less water used in granulation, the smaller the distribution of granular carbon black after granulation, and the powderization rate accounts for more than 50%; when the water used is higher, the distribution of granular carbon black after granulation is larger and not spherical, and the subsequent drying cost is too high. By adjusting the mass ratio of powdered carbon black to water within the above range, the particle size distribution requirements and production costs can be taken into account.

[0059] In a specific embodiment of the present invention, during wetting, a pre-stirring process is performed at a stirring speed of 1000 to 1400 r / min. Furthermore, the pre-stirring process lasts for 1 to 5 minutes.

[0060] During wetting, a certain mass of water is added to a container containing powdered carbon black under stirring conditions, and pre-stirring is performed at a stirring speed of 1000r / min, 1100r / min, 1200r / min, 1300r / min, 1400r / min or any combination thereof, so that the powdered carbon black is in a fluffy state, which is conducive to uniform wetting of water and powdered carbon black. The pre-stirring time can be 1min, 2min, 3min, 4min, 5min or any combination thereof.

[0061] In a specific embodiment of the present invention, the temperature of water is ≥ 60° C. In actual operation, the water used may be deionized water, and the temperature of the water may be 60° C., 70° C., 80° C., etc.

[0062] In actual operation, water can be added by spraying during the granulation process.

[0063] In a specific embodiment of the present invention, the powdered carbon black is any one of acetylene black, furnace black, channel black, lamp black and thermal black.

[0064] The present invention also provides an apparatus for implementing any one of the above-mentioned methods for preparing granular carbon black, such as Figure 1 As shown, it includes a granulation barrel 1 and a stirring paddle 2. The stirring paddle 2 extends into the granulation barrel 1 to stir the material in the granulation barrel 1. The central axis of the granulation barrel 1 does not coincide with the central axis of the stirring paddle 2, that is, eccentric stirring. The granulation barrel 1 can be fixed or supported by a conventional structure such as a frame, which will not be described in detail in the present invention.

[0065] Furthermore, there is a certain angle between the central axis of the granulation barrel 1 and the horizontal plane, that is, the granulation barrel 1 is arranged tilted, wherein the angle may be 60°.

[0066] Another aspect of the present invention provides an electrode, comprising any one of the above-mentioned granular carbon blacks.

[0067] Among them, carbon black is used as a conductive material in the preparation of electrodes. Carbon black can be used as the only conductive material or together with other conductive materials.

[0068] Another aspect of the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator; at least one of the positive electrode and the negative electrode is any one of the above electrodes.

[0069] The powdered carbon black used in the following specific examples and comparative examples is the same as conventional commercially available powdered carbon black.

[0070] Example 1

[0071] Example 1 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0072] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 25 minutes; then stir at a stirring speed of 1500 r / min for 5 minutes; finally, dry at 90°C after discharging.

[0073] Example 2

[0074] Example 2 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0075] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2.1 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1400 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 25 minutes; then stir at a stirring speed of 1500 r / min for 5 minutes; finally, dry at 90°C after discharging.

[0076] Example 3

[0077] Example 3 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0078] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2.5 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2200 r / min for 25 minutes; then stir at a stirring speed of 1500 r / min for 5 minutes; finally, dry at 90°C after discharging.

[0079] Example 4

[0080] Example 4 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0081] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 25 minutes; then stir at a stirring speed of 1200 r / min for 8 minutes; finally, dry at 90°C after discharging.

[0082] Example 5

[0083] Example 5 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0084] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2 kg of 70°C water into the granulation barrel while stirring, stir at a stirring speed of 1000 r / min for 3 minutes; then stir at a stirring speed of 2800 r / min for 15 minutes; then stir at a stirring speed of 1800 r / min for 2 minutes; finally, dry at 90°C after discharging.

[0085] Comparative Example 1

[0086] Comparative Example 1 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0087] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 3 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 25 minutes; then stir at a stirring speed of 1500 r / min for 5 minutes; finally, dry at 90°C after discharging.

[0088] Comparative Example 2

[0089] Comparative Example 2 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0090] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 1.8 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 15 minutes; then stir at a stirring speed of 1500 r / min for 5 minutes; finally, dry the remaining after discharge at 90°C.

[0091] Comparative Example 3

[0092] Comparative Example 3 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0093] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 30 minutes; then stir at a stirring speed of 1500 r / min for 10 minutes; finally, dry at 90°C after discharging.

[0094] Comparative Example 4

[0095] Comparative Example 4 provides a method for preparing granular carbon black, using Figure 1 The equipment shown is prepared, comprising the following steps:

[0096] Add 1 kg of powdered carbon black raw material into the granulation barrel, add 2 kg of water at 60°C into the granulation barrel while stirring, stir at a stirring speed of 1200 r / min for 3 minutes; then stir at a stirring speed of 2400 r / min for 30 minutes; finally, dry the material at 90°C after discharge.

[0097] Comparative Example 5

[0098] Comparative Example 5 provides a method for preparing granular carbon black, which is prepared by a conventional wet horizontal gear hobbing granulator, specifically:

[0099] 1 kg of powdered carbon black raw material was transported to a wet horizontal gear hobbing granulator, and 2.7 kg of deionized water was added for wet granulation. After granulation for 5 minutes, the raw material was taken out and dried at 90°C.

[0100] Comparative Example 6

[0101] The powdered carbon black raw material used in Example 1.

[0102] Experimental Example 1

[0103] The DBP oil absorption value of carbon black was determined by the method of GB / T 14853.6; the particle strength of granular carbon black was determined by the method of GB / T 14853.6; the secondary particle size D50 of carbon black was determined by the method of GB / T 19077.1; the apparent specific volume of carbon black was determined by the method of GB / T3781.6; the particle size distribution of carbon black was determined by sieve screening method (sieve 120 mesh, 20 mesh). The performance data of granular carbon black of Examples 1 to 5 and Comparative Examples 1 to 5 and powdered carbon black of Comparative Example 6 are shown in Table 1.

[0104] Table 1 Performance test results

[0105]

[0106]

[0107]

[0108] As can be seen from Table 1, in the granular carbon black of the present invention, the proportion of granular components with a particle size of less than 0.125 mm is ≤2wt%, which is much lower than the granular carbon black produced by the existing granulation technology in Comparative Example 5, which greatly reduces the pulverization phenomenon of granular carbon black during transportation and processing. At the same time, the particle size distribution of granular carbon black enables small particles of carbon black to fully fill the vacancies between large particles of carbon black, thereby greatly improving the packing density, so that a certain volume of granular carbon black has as many particles as possible, and then it is easier to evenly distribute to electrode materials, resins and / or rubbers during the application process, thereby improving the dispersibility of carbon black in electrode materials, resins and / or rubbers. In addition, from the comparison of apparent specific volume, it can be seen that the apparent specific volume of the granular carbon black of the present invention is reduced, and the packing density is increased, which is consistent with the analysis results of the particle size distribution of the granular carbon black.

[0109] The change rates of the secondary particle size D50 of the powdered carbon black used to prepare granular carbon black in Examples 1-5 before and after granulation are 64.9%, 77.3%, 60.2%, 63.7%, and 71.7%, respectively. It can be seen that the secondary particle size D50 of the granular carbon black is greatly reduced compared to the secondary particle size D50 of the powdered carbon black raw material. In the granulation process of the present invention, the powdered carbon black raw material is repeatedly stirred and sheared by a stirring mechanism to deagglomerate the agglomerate structure of the carbon black, thereby reducing the secondary particle size, thereby making the granular carbon black better dispersed during processing and application, thereby improving dispersibility.

[0110] The change rates of the DBP oil absorption values ​​of the powdered carbon black used to prepare the granulated carbon black in Examples 1-5 before and after granulation are 18.4%, 26.5%, 14.3%, 16.3%, and 22.4%, respectively. It can be seen that the DBP oil absorption value of the granulated carbon black prepared by the present invention is lower than that of the ungranulated powdered carbon black raw material, and the degree of reduction can be controlled within the corresponding range, which shows that although the secondary particle size D50 is greatly reduced during the granulation process of the present invention, the structural damage to the microscopic porous structure is limited, so the impact on the performance of the granulated carbon black is greatly reduced.

[0111] The particle strength of the granular carbon black prepared by the present invention meets certain requirements, and can prevent the granular carbon black from being easily broken during transportation and easily crushed during use and processing, thereby improving the practicality and dispersibility of the granular carbon black.

[0112] Experimental Example 2

[0113] The granular carbon black of Examples 1 to 5 and Comparative Examples 1 to 6 were used to prepare electrode slurries, and the film resistance test was performed, which specifically included the following steps:

[0114] 1. Preparation of electrode slurry

[0115] LiCoO2, polyvinylidene fluoride and granular carbon black were mixed in N-methylpyrrolidone at a mass ratio of 96:2:2 to prepare an electrode slurry, wherein the carbon black was the granular carbon black prepared in Examples 1 to 5 and Comparative Examples 1 to 5.

[0116] 2. Preparation of diaphragm

[0117] The electrode slurry prepared above was coated on a PET film with a thickness of 100 μm on a coating machine, dried at 90° C., and then cut into discs with a diameter of 30 mm.

[0118] 3. Test of diaphragm resistance

[0119] The cut PET disc was placed on the RTS-8 four-probe tester, and the corresponding temperature (23±3℃), humidity (relative humidity ≤30%), PET disc thickness and diameter parameters were set, and the film resistance was tested by adjusting the current. The test results are shown in Table 2.

[0120] Table 2 Test results of different film resistances

[0121]

[0122] As can be seen from the above table, the membrane resistance of the electrode slurry prepared using the granular carbon black of the embodiment of the present invention is significantly lower than the membrane resistance of the electrode slurry prepared using the granular carbon black of the comparative example. It can be confirmed that the method of the present invention is used to granulate the powdered carbon black so that the secondary particle size of the obtained granular carbon black meets the corresponding range and has a certain particle size distribution, which can make the granular carbon black well dispersed between the electrode active materials, thereby increasing the contact between the electrode active materials and the carbon black, and improving the conductivity of the slurry and the electrode.

[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. Granular carbon black, characterized in that The particle size distribution range of the granular carbon black is as follows: The proportion of granular components with a particle size of less than 0.125 mm is ≤ 2wt%, the proportion of granular components with a particle size of 0.125 to 0.85 mm is 18wt% to 60wt%, and the proportion of granular components with a particle size of more than 0.85 mm is 40wt% to 80wt%; The secondary particle size D50 of the granular carbon black is 2.0 to 3.51 μm; The DBP oil absorption value of the granular carbon black is X1, and the DBP oil absorption value of the powdered carbon black obtained by granulating the granular carbon black is X2, and X1 and X2 satisfy: (X2-X1) / X2 is 14.3% to 26.5%; The apparent specific volume of the granular carbon black is 3.2 to 3.4 mL / g; The secondary particle size D50 of the granular carbon black is Y1, and the secondary particle size D50 of the powdered carbon black obtained by granulation is Y2, and Y1 and Y2 satisfy: (Y2-Y1) / Y1 is 60.2% to 77.3%; The particle strength of the granular carbon black is ≤5.3 gf / piece.

2. The granular carbon black according to claim 1, characterized in that The particle strength of the granular carbon black is 4.6 to 5.3 gf / piece.

3. The granular carbon black according to claim 1, characterized in that The raw material of the granular carbon black is acetylene black.

4. The method for preparing granular carbon black according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: wetting the powdered carbon black with water, and then wet granulating and drying the powdered carbon black; In the wet granulation, the stirring speed is firstly 2200-2800 r / min for 15-25 min, and then the stirring speed is 1200-1800 r / min for 2-8 min. The mass ratio of the powdered carbon black to the water is 1:(2-2.5).

5. The method for preparing granular carbon black according to claim 4, characterized in that: During the wetting, a pre-stirring treatment is performed at a stirring speed of 1000 to 1400 r / min.

6. The method for preparing granular carbon black according to claim 5, characterized in that: The pre-mixing treatment time is 1 to 5 minutes.

7. The method for preparing granular carbon black according to claim 4, characterized in that: The temperature of the water is ≥60°C.

8. The method for preparing granular carbon black according to claim 4, characterized in that: The powdered carbon black is acetylene carbon black.

9. An electrode, characterized in that: The invention comprises the granular carbon black as described in any one of claims 1 to 3 or the granular carbon black prepared by the preparation method as described in any one of claims 4 to 8.

10. A secondary battery, characterized in that: It comprises a positive electrode, a negative electrode, an electrolyte and a separator; at least one of the positive electrode and the negative electrode is the electrode according to claim 9.

Citation Information

Patent Citations

  • Granular conductive carbon black and production method thereof

    CN110437650A

  • Granular acelylene black, its production method and use

    CN1304961A

  • Carbon black pelleting

    GB1280856A

  • Carbon black

    GB1390123A

  • Carbon black and ink composition

    JP2004269572A