A method for recovering copper, tin, zinc and lead from tin bronze
By using stepwise vacuum distillation and cuprous sulfide reaction, the problem of efficient separation of copper, tin, zinc and lead in tin bronze waste was solved, achieving recovery with low impurity content, simplifying the process and reducing environmental pollution.
Patent Information
- Application Number
- CN202211126984.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-16
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-09-16
AI Technical Summary
Existing technologies for recovering copper, tin, zinc, and lead from tin bronze waste suffer from problems such as complex processes, severe environmental pollution, and high impurity content.
The stepwise vacuum distillation method is adopted. First, tin bronze is heated and melted for vacuum distillation to separate the lead-zinc alloy. Then, it is mixed with cuprous sulfide and reacted under vacuum conditions to generate tin sulfide. Finally, copper is recovered by blowing in air.
It achieves efficient separation of copper, tin, zinc, and lead, reduces environmental pollution, lowers impurity content, and simplifies the process.
Smart Images

Figure CN117758054B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of tin bronze recycling, and in particular to a method for recovering copper, tin, zinc and lead from tin bronze. Background Technology
[0002] Tin bronze is an alloy with copper and tin as the main alloying elements. It has high strength, corrosion resistance, and excellent casting properties. Industrial tin bronze generally contains 3 to 14 wt% tin. In addition, it also contains small amounts of metals such as lead and zinc. It is mainly used to make elastic components and wear-resistant parts.
[0003] Tin bronze scrap refers to the offcuts, expired or unusable metal scraps generated during industrial production using tin bronze as raw material. Examples include discarded forgings, tin-plated copper wire, and welding waste from electronic components. With the gradual depletion of metal ore reserves, copper, tin, zinc, and lead can be recovered from tin bronze scrap, enabling continuous metal recycling, reducing the extraction of primary resources, saving significant energy, and promoting ecological civilization and economic development.
[0004] Currently, the recovery of various metal components from tin bronze waste mainly employs wet and pyrometallurgical processes. Chinese invention patent application number 201610668478.0 discloses a comprehensive recycling process for tin-copper-gold-silver waste. This process involves ball milling, drying, roasting, and pulverizing the waste to ensure thorough separation of tin, copper, gold, and silver elements. Subsequently, the waste undergoes layered extraction and separation using acids, alkalis, or other reagents, recovering copper, tin, silver, and gold sequentially. While this process offers relatively high precision, it is complex. The addition of acid and alkali solutions during recycling increases equipment corrosion. Ball milling can easily introduce new metallic impurities, and wastewater is generated during solid-liquid separation and electrolysis.
[0005] Chinese invention patent application number 201710802746.8 discloses a method for separating copper-tin alloys using recycled tin sulfide. The method involves melting the copper-tin alloy under normal pressure, adding tin sulfide, cooling, and removing slag to obtain crude tin containing less than 0.1% Cu and sulfur slag. Metallic tin is selectively added to or not added to the sulfur slag, and the material is then vacuum distilled to obtain metallic copper and tin sulfide. This invention uses tin sulfide for copper-tin separation, and the separation process is a full pyrometallurgical method, which does not generate wastewater or waste gas. However, the amount of tin added before vacuum distillation is often difficult to control; if too much tin is added, the distillation residue will form a tin-copper alloy.
[0006] Chinese Patent CN109338109B discloses a method for separating valuable metals from high-zinc, lead, and tin scrap copper, belonging to the field of scrap copper resource utilization technology. Scrap copper raw materials with high zinc, lead, and tin content have a copper content of 75-85%. The main processing steps include screening, crushing, mixing, and atmospheric / controlled-pressure high-temperature treatment. After crushing, the raw material is treated in a high-temperature furnace at atmospheric pressure (1400-1800℃) or controlled pressure (0.1-0.5 atm) (1000-1500℃) with the addition of cuprous sulfide. After cooling, the volatiles yield zinc, lead, and tin or their compounds. The treated scrap copper has significantly reduced zinc, lead, and tin impurities and can be used to produce pure copper or copper alloys, achieving comprehensive utilization of scrap copper resources. This method can separate copper from scrap copper, but components such as zinc, lead, and tin in the scrap copper form elements or compounds mixed in volatiles. During the separation process, waste gas is easily generated and escapes, polluting the environment. The oxygen content in the reaction vessel is high, the metal components are easily oxidized, the volatilization temperature is high under normal or slightly negative pressure, the reaction time of lead and tin with cuprous sulfide is long, and the impurity content in the recovered copper is still high. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to provide a method for recovering copper, tin, zinc and lead from tin bronze, which addresses the shortcomings of the existing technology. The method involves the stepwise recovery of zinc, lead, copper and tin, is environmentally friendly, has a short reaction time, and results in low impurity content in the recovered copper.
[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for recovering copper, tin, zinc and lead from tin bronze, comprising the following steps:
[0009] S1. Recovery of lead-zinc alloy from tin bronze: After heating and melting tin bronze, vacuum distillation A is carried out to obtain volatile A and residue A. Volatile A is condensed and recovered to obtain lead-zinc alloy.
[0010] S2, Tin recovery: Mix the residue A obtained in S1 with cuprous sulfide evenly, and then perform vacuum distillation B on the mixed material. The volatile substance B is obtained by condensation, and the remaining substance is residue B.
[0011] S3, Copper Recovery: The residue B obtained in S2 is smelted in air to recover crude copper.
[0012] Lead and zinc have significantly different volatility compared to copper and tin. This invention separates lead and zinc through stepwise distillation, avoiding the influence of lead and zinc components on the amount of cuprous sulfide added during copper-tin separation, and also preventing the mixing of tin and lead-zinc components after volatilization. This invention first separates the low-boiling-point components of lead and zinc, and then separately separates and recovers lead, zinc, copper, and tin. The vacuum distillation method does not generate waste gas, making it environmentally friendly, and the recovered metal components do not oxidize. Copper and tin have very similar volatility, making separation under normal pressure difficult. This invention, under vacuum conditions, allows the spontaneous reaction of tin with cuprous sulfide to form stannous sulfide. The reaction temperature is lower, the time is shorter, and the volatility difference between stannous sulfide and copper is greater, resulting in more thorough separation of tin and copper, and a lower impurity content in the recovered copper.
[0013] In S2, tin is converted into tin sulfide, then volatilizes and condenses to obtain volatile product B. The main component of volatile product B is tin sulfide, and the residue B is mainly copper and excess unreacted cuprous sulfide.
[0014] If lead and zinc are not separated first and tin is recovered directly, the amount of lead and zinc will affect the amount of cuprous sulfide added later. The separated volatiles are a mixture of tin, lead and zinc, and the recovered copper has a high impurity content.
[0015] In a preferred embodiment of the present invention, the temperature of vacuum distillation B in S2 is 1200-1400°C, the pressure is 10-40 Pa, and the distillation time is 20-40 min.
[0016] Under this vacuum environment and temperature, the tin component and cuprous sulfide in residue A (mainly a copper-tin alloy) spontaneously react to form tin sulfide and copper. The spontaneous reaction occurs at temperatures above 1000℃, and the higher the temperature, the faster the spontaneous reaction rate. Lower pressure results in lower spontaneous reaction temperatures and lower boiling points for component volatilization. However, if the temperature is too high, a small amount of copper component will also volatilize during vacuum distillation. If the temperature is too low, cuprous sulfide and copper components are difficult to melt or have poor fluidity after melting. If the pressure is too high, the boiling points of the separated components increase, and the required separation temperature also increases. If the pressure is too low, achieving a vacuum system becomes more difficult. If the distillation time is too long, a small amount of copper component will enter the volatiles; if the distillation time is too short, the separation between components is incomplete.
[0017] In a preferred embodiment of the present invention, the residue A in S2 is mixed with cuprous sulfide in a way that the mixture is melted and then mixed evenly.
[0018] After melting, residue A (mainly composed of copper-tin alloy) can be more easily and evenly mixed with cuprous sulfide.
[0019] In a preferred embodiment of the present invention, residue A and cuprous sulfide are added to the melting pool simultaneously in S2. Residue A is a molten solution, and cuprous sulfide is in the form of lumps or powder with a particle size of less than 20 mm.
[0020] The residue A obtained from vacuum distillation A is initially in a liquid state and directly enters the vacuum distillation process B. It is necessary to avoid residue A cooling down to a solid state before entering S2 for heating. Residue A and cuprous sulfide must be mixed thoroughly; mixing liquid residue A with cuprous sulfide is easier than mixing solid residues together.
[0021] In a preferred embodiment of the present invention, the mixing of residue A and cuprous sulfide in S2 is carried out by introducing inert gas into the molten pool to agitate it or by mechanical stirring; preferably, the mixing of residue A and cuprous sulfide in S2 is carried out by introducing inert gas into the molten pool to agitate it.
[0022] The purpose of introducing inert gas to agitate the mixture is to ensure more thorough mixing of the liquid residue A with cuprous sulfide, while preventing oxidation of the components. Uniform mixing facilitates the reaction of tin with cuprous sulfide to form tin sulfide and copper during subsequent vacuum distillation. If the reaction is uneven, residual tin components will remain during vacuum distillation.
[0023] In a preferred embodiment of the present invention, the molar mass of cuprous sulfide in S2 is 1.5 to 2.0 times the molar mass of Sn in residue A.
[0024] The amount of cuprous sulfide added in S2 is 1.5 to 2.0 times the theoretical amount required for the reaction of tin in residue A with cuprous sulfide to form tin sulfide (i.e., reaction ①). In this process, cuprous sulfide needs to be in excess to ensure that all the tin in residue B participates in the reaction to form tin sulfide, thus achieving full sulfidation of the tin and realizing the purpose of tin recovery.
[0025] Reaction ①
[0026] In a preferred embodiment of the present invention, the method for recovering copper, tin, zinc and lead from tin bronze further includes a lead-zinc alloy separation and recovery step: the lead-zinc alloy in S1 is separated and recovered to obtain crude lead and crude zinc respectively.
[0027] In a preferred embodiment of the present invention, the lead-zinc alloy is separated and recycled by vacuum distillation or by pyrometallurgical smelting, preferably by vacuum distillation.
[0028] Vacuum distillation separates different components by utilizing their different boiling points. Vacuum conditions can also lower the boiling point temperature to a certain extent, resulting in a lower separation temperature. At the same time, no new impurities are introduced during the separation process, and no pollutants such as wastewater or waste gas are generated, making it more environmentally friendly.
[0029] In a preferred embodiment of the present invention, the temperature of vacuum distillation A in S1 is 1100-1200°C, the pressure is 10-40 Pa, and the distillation time is 20-40 min.
[0030] The raw materials need to be melted before distillation. Vacuum conditions affect the boiling point of the materials, but have little effect on their melting point. Therefore, the distillation temperature must be controlled above the melting point of the raw materials, which is around 1050℃. Through a vacuum environment and at a certain temperature, lead and zinc, and copper and tin, are separated from the raw materials. Lead and zinc are recovered as volatiles, while copper and tin are mainly found in the residue. If the temperature is too high, a small amount of copper and tin will also enter the volatiles; if the temperature is too low, the raw material's fluidity deteriorates, and it may even solidify. If the pressure is too high, the distillation separation rate slows down; if the pressure is too low, achieving a vacuum system becomes more difficult. If the distillation time is too long, a small amount of copper and tin will enter the volatiles; if the distillation time is too short, the separation between components is incomplete.
[0031] In a preferred embodiment of the present invention, the blowing temperature of residue B in S3 is 1100-1400°C, preferably 1200-1300°C.
[0032] By smelting the copper component in an air atmosphere, excess cuprous sulfide is converted into copper and sulfur dioxide. The sulfur dioxide can be used to produce acid, thus achieving copper recovery. At excessively high temperatures, the reaction is more vigorous, and a small amount of copper component will enter the volatiles, and energy consumption is high. At lower temperatures, the component has poor fluidity after melting.
[0033] This invention utilizes multiple vacuum distillations to separate zinc, lead, and tin from tin bronze waste. Under different temperatures and pressures, low-boiling-point components such as lead and zinc in the tin bronze waste first volatilize from the alloy, yielding volatile A and residue A. Volatile A can be further separated and recovered to obtain crude lead and crude zinc through vacuum distillation or pyrometallurgical smelting. Residue A mainly consists of copper, tin, and other non-volatile metallic components. If residue A is directly melted and vacuum distilled, the boiling points of copper and tin are very close, making them difficult to separate. However, when cuprous sulfide is added and melted together with residue A, and mixed evenly, under vacuum distillation conditions of a certain negative pressure and high temperature, tin and cuprous sulfide can spontaneously react to produce tin sulfide and copper. The volatility of tin sulfide differs significantly from that of copper. During vacuum distillation, the tin sulfide volatilizes and condenses, yielding volatile compound B, whose main component is tin sulfide. Residue B mainly consists of copper and excess unreacted cuprous sulfide, which can be smelted in air to recover crude copper.
[0034] In this invention, the copper-tin components and cuprous sulfide need to be mixed evenly to facilitate the reaction of tin and cuprous sulfide under vacuum conditions. Based on the different volatility of tin sulfide and copper, the temperature and pressure of vacuum distillation are controlled to make the separation of copper and tin components more thorough.
[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0036] (1) Tin bronze waste is vacuum distilled in two stages. Through vacuum distillation A, low-boiling-point components such as lead and zinc in tin bronze waste are volatilized, condensed and collected, and then lead and zinc are recovered separately. The process is simple, easy to operate and the separation is thorough.
[0037] (2) The tin recovery process is simplified and the reaction is integrated. Residue A and cuprous sulfide are first melted and mixed evenly. In the negative pressure and high temperature environment of vacuum distillation B, cuprous sulfide itself does not decompose and can spontaneously react with the tin in residue A to generate copper and tin sulfide. The saturated vapor pressures of tin and copper are very close. When tin is converted into tin sulfide, the saturated vapor pressure increases and the boiling point decreases. By using vacuum distillation, tin is continuously converted into tin sulfide and volatilized and condensed, realizing the separation and recovery of tin and copper.
[0038] (3) The entire process is carried out in a high-temperature or enclosed space, with no wastewater generated and less waste gas and waste residue generated, which is more environmentally friendly.
[0039] (4) The present invention can achieve high-precision separation of copper, tin, zinc and lead from tin bronze waste. The total content of Pb and Zn in the vacuum distillation residue A is <0.01%, and the content of Sn in the vacuum distillation residue B is <0.2%. Attached Figure Description
[0040] Figure 1 This is a process flow diagram of an embodiment of the present invention. Detailed Implementation
[0041] All the following embodiments use the same tin bronze scrap as raw material, whose main components are: Cu 93.23%, Sn 3.89%, Zn 2.76%, Pb 0.03%. The shape is 10*30mm sheet.
[0042] Example 1:
[0043] like Figure 1 As shown, this embodiment includes the following steps:
[0044] Step 1: After melting the tin bronze waste, vacuum distillation A is carried out at a temperature of 1100℃ and a pressure of 10Pa for 30 minutes to obtain volatile A and residue A. Volatile A is condensed and collected to obtain lead-zinc alloy. Copper, tin and other elements remain in residue A. The copper, tin, zinc and lead composition of residue A is shown in Table 1.
[0045] Step 2: The condensed volatile A is separated by vacuum distillation at a temperature of 650℃ and a pressure of 20Pa, and crude lead and crude zinc are recovered.
[0046] Step 3: Melt residue A together with cuprous sulfide at a melting temperature of 1150℃, mix thoroughly, and purge nitrogen into the molten pool to ensure uniform mixing. Based on the copper and tin composition of residue A, the amount of cuprous sulfide added is 1.5 times the theoretical amount required for the reaction of tin in residue A with cuprous sulfide to generate tin sulfide (i.e., reaction ①). The mixed material is then subjected to vacuum distillation B at a temperature of 1200℃, a pressure of 10Pa, and a distillation time of 30min. Tin is converted into tin sulfide, which is then volatilized and condensed to obtain volatiles B and residue B. The main component of volatiles B is tin sulfide, and the main components of residue B are copper and excess unreacted cuprous sulfide. The copper and tin composition of residue B is shown in Table 1.
[0047] Reaction ①
[0048] Step 4, Copper Recovery: The residue B obtained in Step 3 is smelted in air at a temperature of 1200-1300℃ to recover crude copper.
[0049] Table 1:
[0050]
[0051] Note: Content <0.01% indicates not detected.
[0052] Example 2:
[0053] Step 1: After melting the tin bronze waste, vacuum distillation A is carried out at a temperature of 1100℃ and a pressure of 40Pa for 30 minutes to obtain volatile A and residue A. Volatile A is condensed and collected to obtain lead-zinc alloy. Copper, tin and other elements remain in residue A. The copper, tin, zinc and lead composition of residue A is shown in Table 2.
[0054] Step 2: The condensed volatile A is separated by vacuum distillation at a temperature of 650℃ and a pressure of 20Pa, and crude lead and crude zinc are recovered.
[0055] Step 3: Melt residue A together with cuprous sulfide at a melting temperature of 1150℃, mix thoroughly, and purge nitrogen into the molten pool to ensure uniform mixing. Based on the copper and tin composition of residue A, the amount of cuprous sulfide added is 1.5 times the theoretical amount required for the reaction of tin in residue A with cuprous sulfide to form tin sulfide (i.e., reaction ①). The mixed material is then subjected to vacuum distillation B at a temperature of 1400℃, a pressure of 40Pa, and a distillation time of 30min. Tin is converted into tin sulfide, which is then volatilized and condensed to obtain volatiles B and residue B. The main component of volatiles B is tin sulfide, and the main components of residue B are copper and excess unreacted cuprous sulfide. The copper and tin composition of residue B is shown in Table 2.
[0056] Reaction ①
[0057] Step 4, Copper Recovery: The residue B obtained in Step 3 is smelted in air at a temperature of 1200-1300℃ to recover crude copper.
[0058] Table 2:
[0059]
[0060] Note: Content <0.01% indicates not detected.
[0061] Example 3:
[0062] Step 1: After melting the tin bronze waste, vacuum distillation A is carried out at a temperature of 1200℃ and a pressure of 20Pa for 30 minutes to obtain volatile A and residue A. Volatile A is condensed and collected to obtain lead-zinc alloy. Copper, tin and other elements remain in residue A. The copper, tin, zinc and lead composition of residue A is shown in Table 3.
[0063] Step 2: The condensed volatile A is separated by vacuum distillation at a temperature of 650℃ and a pressure of 20Pa, and crude lead and crude zinc are recovered.
[0064] Step 3: Melt residue A together with cuprous sulfide at a melting temperature of 1150℃, mix thoroughly, and purge nitrogen into the molten pool to ensure uniform mixing. Based on the copper and tin composition of residue A, the amount of cuprous sulfide added is 2.0 times the theoretical amount required for the reaction of tin in residue A with cuprous sulfide to generate tin sulfide (i.e., reaction ①). The mixed material is then subjected to vacuum distillation B at a temperature of 1300℃, a pressure of 20Pa, and a distillation time of 30min. Tin is converted into tin sulfide, which is then volatilized and condensed to obtain volatiles B and residue B. The main component of volatiles B is tin sulfide, and the main components of residue B are copper and excess unreacted cuprous sulfide. The copper and tin composition of residue B is shown in Table 3.
[0065] Reaction ①
[0066] Step 4, Copper Recovery: The residue B obtained in Step 3 is smelted in air at a temperature of 1200-1300℃ to recover crude copper.
[0067] Table 3:
[0068]
[0069]
[0070] Note: Content <0.01% indicates not detected.
[0071] The above description is merely an embodiment of the present invention and is not intended to limit the scope of the invention. After reading this invention, any modifications of the invention by those skilled in the art in various equivalent forms fall within the scope defined by the appended claims.
Claims
1. A method for recovering copper, tin, zinc, and lead from tin bronze, characterized in that... Includes the following steps: S1. Recovery of lead-zinc alloy from tin bronze: After heating and melting tin bronze, vacuum distillation A is carried out to obtain volatile A and residue A. Volatile A is condensed and recovered to obtain lead-zinc alloy. S2, Tin recovery: Mix the residue A obtained in S1 with cuprous sulfide evenly, and then perform vacuum distillation B on the mixed material. The volatile substance B is obtained by condensation, and the remaining substance is residue B. S3, Copper Recovery: The residue B obtained in S2 is smelted in air to recover crude copper; In S2, the temperature for vacuum distillation of B is 1200~1400℃, the pressure is 10~40Pa, and the distillation time is 20-40min.
2. The method for recovering copper, tin, zinc, and lead from tin bronze according to claim 1, characterized in that, The residue A in S2 is mixed evenly with cuprous sulfide by melting and then mixing.
3. The method for recovering copper, tin, zinc, and lead from tin bronze according to claim 2, characterized in that, In S2, residue A and cuprous sulfide are added to the molten pool at the same time and melted. Residue A is a molten solution, and cuprous sulfide is in the form of lumps or powder with a particle size of less than 20 mm.
4. The method for recovering copper, tin, zinc, and lead from tin bronze according to claim 2, characterized in that, The mixing of residue A and cuprous sulfide in S2 is achieved by either blowing inert gas into the molten pool to disturb the mixture or by mechanical stirring.
5. The method for recovering copper, tin, zinc, and lead from tin bronze according to claim 4, characterized in that, The mixing of residue A and cuprous sulfide in S2 is achieved by turbulence of inert gas into the molten pool.
6. The method for recovering copper, tin, zinc, and lead from tin bronze according to any one of claims 1-5, characterized in that, The molar amount of cuprous sulfide in S2 is 1.5 to 2.0 times the molar amount of Sn in residue A.
7. The method for recovering copper, tin, zinc, and lead from tin bronze according to any one of claims 1-5, characterized in that, It also includes a lead-zinc alloy separation and recycling step: the lead-zinc alloy in S1 is separated and recycled to obtain crude lead and crude zinc respectively.
8. The method for recovering copper, tin, zinc, and lead from tin bronze according to claim 7, characterized in that, Lead-zinc alloys are separated and recycled using vacuum distillation or pyrometallurgical smelting.
9. The method for recovering copper, tin, zinc, and lead from tin bronze according to any one of claims 1-5, characterized in that, In S1, the temperature for vacuum distillation of A is 1100~1200℃, the pressure is 10~40Pa, and the distillation time is 20~40min.
10. The method for recovering copper, tin, zinc, and lead from tin bronze according to any one of claims 1-5, characterized in that, The blowing temperature of residue B in S3 is 1100~1400℃.
11. The method for recovering copper, tin, zinc, and lead from tin bronze according to any one of claims 1-5, characterized in that, The blowing temperature of residue B in S3 is 1200~1300℃.
Citation Information
Patent Citations
Comprehensive recovery process for tin-copper-gold-silver waste materials
CN106282571A
A method for separating valuable metals from high-zinc, lead, tin scrap copper.
CN109338109B
Process for recovering copper and zinc and tin and lead by utilizing side blown converter at the bottom
CN102925702A
Method for removing lead, zinc, arsenic, antimony, bismuth and tin from copper matte
CN103397200A
Method for separating copper-tin alloy by circularly using stannous sulfide
CN107574307A