Small convex electrical steel and its preparation method and application

Through the continuous casting and rolling process of thin slabs and the self-learning model, the rolling parameters are optimized, combined with alternating hot rolling and layer cold treatment, the problem of hot rolling convexity control of non-oriented electrical steel is solved, and the preparation of low-convexity electrical steel is realized to ensure that The goodness of surface quality after acid rolling and the controllability of the rolling unit are achieved.

CN117772794BActive Publication Date: 2024-11-12HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311735491.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-12
Estimated Expiration
2043-12-15

Smart Images

  • Figure CN117772794B_ABST
    Figure CN117772794B_ABST
Patent Text Reader

Abstract

The present application discloses a small-convex electrical steel and its preparation method and application. A preparation method for small-convex electrical steel, the preparation method comprising: performing alternating hot continuous rolling on the electrical steel ingot and the non-electrical steel ingot to obtain the small-convex electrical steel; wherein the automation control system comprises a basic automation system and a secondary process control system, the secondary process control system comprises a self-learning model, the self-learning model is used to optimize the rolling parameters including working roll shifting, bending roll force dynamics and rolling temperature according to the physical and chemical data of the electrical steel and the non-electrical steel, the rolling parameters and the functional relationship of the convexity after rolling. According to the embodiment of the present application, the convexity of the hot-rolled substrate of the electrical steel can be reduced, so that the local high point of the cross section of the hot-rolled substrate is ≤10μm, and the surface quality after acid rolling is normal without rib defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of electrical steel, and in particular relates to a small-convex electrical steel and a preparation method and application thereof. Background Art

[0002] Electrical steel is widely used in household electrical motors and small transformers. With the development of high speed and miniaturization of motors, higher requirements are placed on the performance of non-oriented electrical steel. Among them, the transverse plate difference is an important indicator of non-oriented electrical steel, which directly affects the performance of the core after lamination.

[0003] The convexity of hot rolled coil directly affects the transverse plate difference after pickling. However, small convexity control will lead to local high points in the cast non-oriented electrical steel and rib defects after pickling. Summary of the invention

[0004] The embodiment of the present application provides a small-convex electrical steel and a preparation method and application thereof, which can reduce the convexity of the hot-rolled substrate of the electrical steel so that the local high point of the cross section of the hot-rolled substrate is ≤10μm, and the surface quality after acid rolling is normal without rib defects.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing small-convex electrical steel, comprising an automated control system and a casting and rolling device, and adopting a thin slab continuous casting and rolling process for production, the preparation method comprising: refining electrical steel molten steel and non-electrical steel molten steel to obtain refined electrical steel molten steel and refined non-electrical steel molten steel, wherein the refined electrical steel molten steel contains the following components by mass percentage: 0.000%≤C≤0.006%, 0.3%≤Si≤0.9%, 0.2%≤Mn≤0.5%, 0.01%≤P≤0.1%, 0.000%≤S≤0.006%, 0.2%≤Al≤0.5%, 0.0000%≤N≤0.0050% and 0.0000%≤Ti≤0.0050%, and the remainder is iron and unavoidable trace elements;

[0006] Continuously casting the refined electrical steel molten steel and the refined non-electrical steel molten steel respectively to obtain electrical steel ingots and non-electrical steel ingots;

[0007] Alternately hot rolling electrical steel ingots and non-electrical steel ingots to obtain small crown electrical steel;

[0008] Among them, the automation control system includes a basic automation system and a secondary process control system. The secondary process control system includes a self-learning model. The self-learning model is used to optimize the rolling parameters including working roll shifting, bending roll force dynamics and rolling temperature according to the physical and chemical data of electrical steel and non-electrical steel, rolling parameters and the functional relationship between the convexity after rolling.

[0009] In any embodiment of the present application, in the step of alternately hot rolling the electrical steel ingot and the non-electrical steel ingot, the step comprises:

[0010] The electrical steel ingots and non-electrical steel ingots are placed in the first swing heating furnace and the second swing heating furnace respectively. The outlet of the first swing heating furnace is connected to the hot rolling mill. The electrical steel ingots or non-electrical steel ingots are transported from the second swing heating furnace to the first swing heating furnace through the swing section of the heating furnace for alternating hot rolling.

[0011] In any embodiment of the present application, the physicochemical data of the electrical steel and the non-electrical steel include the composition of the steel billet.

[0012] In any embodiment of the present application, in the swing heating furnace, the heating temperature of the electrical steel ingot is 1100-1160°C, and the furnace discharge temperature is 1020-1080°C.

[0013] In any embodiment of the present application, the self-learning model includes short-term learning and long-term learning.

[0014] In any embodiment of the present application, short-term learning includes: first inputting the physicochemical data, rolling parameters and convexity after rolling of steel billets with different furnace numbers into the model, training the model to obtain the functional relationship between the physicochemical data of the steel billet, rolling parameters and convexity, and then inputting the set convexity value and the physicochemical data of the steel billet. The model derives the corresponding rolling parameters based on the functional relationship obtained by training, and then adjusts and implements them through the basic automation system; distinguishing the slabs in the first swinging heating furnace and the second swinging heating furnace, and learning the data of the corresponding heating furnace for each.

[0015] In any embodiment of the present application, long-term learning includes: first inputting the physicochemical data, rolling parameters and convexity after rolling of steel billets of different steel grades into the model, training the model to obtain the functional relationship between the physicochemical data of the steel billet, the rolling parameters and the convexity, and then inputting the set convexity value and the physicochemical data of the steel billet. The model derives the corresponding rolling parameters based on the functional relationship obtained through training, and then adjusts and implements them through the basic automation system; subdivides the physicochemical data and rolling parameters of the steel billet, divides them into small intervals, and continuously optimizes the model data.

[0016] In any embodiment of the present application, in the step of refining electrical steel molten steel and non-electrical steel molten steel, the electrical steel molten steel is obtained by sequentially processing through a blast furnace, KR, a converter and a RH furnace, and the non-electrical steel molten steel is obtained by sequentially processing through a blast furnace, KR, a converter and a RH furnace.

[0017] In any embodiment of the present application, in the step of performing alternating hot rolling on electrical steel ingots and non-electrical steel ingots to obtain small-convex electrical steel, the alternating hot rolling is performed using a seven-stand finishing mill.

[0018] In any embodiment of the present application, the step of alternately hot-rolling the electrical steel ingot and the non-electrical steel ingot to obtain the small-convex electrical steel further includes the steps of layer cooling treatment and coiling treatment, wherein the coiling temperature is 600-700°C.

[0019] In any embodiment of the present application, the alternating hot rolling further includes pickling.

[0020] In a second aspect, an embodiment of the present application provides a small convex electrical steel.

[0021] A small convex electrical steel is obtained by the above preparation method.

[0022] In any embodiment of the present application, in the small crown electrical steel, the average crown is 20-21 μm.

[0023] In any embodiment of the present application, in the small-convex electrical steel, the proportion of the convexity ≤25 μm is 82%-93%, and the proportion of the convexity ≤30 μm is 95%-100%.

[0024] In a third aspect, an embodiment of the present application provides an application of a small-convex electrical steel in motors and electronics.

[0025] An application of small-convex electrical steel in motors and electronics, wherein the small-convex electrical steel is selected from the small-convex electrical steel obtained by the above-mentioned preparation method or the above-mentioned small-convex electrical steel.

[0026] The small convex electrical steel and its preparation method and application in the embodiment of the present application can reduce the convexity of the hot-rolled substrate of the electrical steel without shortening the hot-rolling unit, so that the local high point of the cross section of the hot-rolled substrate is ≤10μm. By using alternating rolling of electrical steel and other steel types and a self-learning model, the roll shifting amplitude can be adjusted to reduce the uneven wear of the local rolls, ensure the controllable cross-sectional shape of the entire rolling unit, and ensure that the surface quality after pickling is normal without rib defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solution of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0028] Figure 1 A schematic diagram of the smelting process for this application;

[0029] Figure 2 An example is shown Figure 1 A partial enlarged view of the continuous casting area;

[0030] Figure 3Schematic diagram of the hot rolling process of this application. DETAILED DESCRIPTION

[0031] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the scheme of the present application will be further described below. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present application may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present application, rather than all of the embodiments.

[0033] Hereinafter, the small convex electrical steel of the present application, its preparation method and application implementation methods are specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0034] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0035] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0036] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0037] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0038] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0039] Unless otherwise specified, this application adopts conventional test methods or test methods recommended by the instrument.

[0040] The transverse plate difference refers to the difference between the maximum thickness and the minimum thickness in the width direction of the same plate. The smaller the convexity of the hot-rolled substrate of non-oriented electrical steel, the smaller the transverse plate difference. In the rolling process of non-oriented electrical steel, due to the weak transverse flow characteristics of the metal in the cold rolling stage, in order to avoid wave defects, the cross-sectional shape of the strip cannot be greatly changed in the cold rolling stage. Therefore, the transverse plate difference is mainly determined by the cross-sectional shape of the hot-rolled substrate, that is, the smaller the convexity of the hot-rolled substrate, the smaller the cold-rolled transverse plate difference.

[0041] The present application reduces the convexity of the hot-rolled substrate without affecting the rolling rhythm by adjusting the rolling plan and optimizing the system control model.

[0042]

Preparation method

[0043] The embodiment of the present application provides a preparation method of small-convex electrical steel, including an automatic control system and a casting and rolling device, and adopts a thin slab continuous casting and rolling process for production. The preparation method comprises: refining electrical steel molten steel and non-electrical steel molten steel to obtain refined electrical steel molten steel and refined non-electrical steel molten steel, wherein the refined electrical steel molten steel contains the following components in mass percentage: 0.000%≤C≤0.006%, 0.3%≤Si≤0.9%, 0.2%≤Mn≤0.5%, 0.01%≤P≤0.1%, 0.000%≤S≤0.006%, 0.2%≤Al≤0.5%, 0.0000%≤N≤0.0050% and 0.0000%≤Ti≤0.0050%, the rest are iron and inevitable trace elements; the refined electrical steel molten steel and the refined non-electrical steel molten steel are continuously cast and poured respectively to obtain electrical steel ingots and non-electrical steel ingots; the electrical steel ingots and non-electrical steel ingots are alternately hot-rolled to obtain small convex electrical steel; wherein, the automation control system includes a basic automation system and a secondary process control system, the secondary process control system includes a self-learning model, and the self-learning model is used to optimize the rolling parameters including work roll shifting, bending roll force dynamics and rolling temperature according to the physical and chemical data of electrical steel and non-electrical steel, rolling parameters and the functional relationship of the convexity after rolling. The basic automation system is mainly composed of PLC (programmable logic controller) and DCS (distributed control system), which collects instrument data and equipment status signals for equipment logic control and loop control (control of switch quantity and loop control of simple physical parameters that can be continuously measured, such as temperature, pressure and flow), and transmits data and signals to the secondary process control system. In addition, the basic automation system receives the setting data of the secondary process control system and controls the equipment to achieve the control target according to these setting data. The secondary process control system refers to the part with a higher functional level in the automation control system, which is used to realize more complex control functions. For example, the target hit control of the finished product and semi-finished product manufacturing process in the steel production process, such as the coil thickness control of the hot rolling production line, the terminal molten steel chemical composition and terminal temperature control of the steelmaking converter blowing, requires the use of the mathematical model in the secondary process control system for control, thereby greatly improving the hit rate of the control target. Non-electrical steel includes at least one of carbon structural steel, ordinary cold-rolled steel and alloy structural steel.

[0044] In some embodiments, the step of performing alternating hot rolling on the electrical steel ingot and the non-electrical steel ingot comprises: placing the electrical steel ingot and the non-electrical steel ingot in a first swing heating furnace and a second swing heating furnace respectively, the outlet of the first swing heating furnace is connected to the hot rolling mill, and the electrical steel ingot or the non-electrical steel ingot is transported from the second swing heating furnace to the first swing heating furnace through the swing section of the heating furnace for alternating hot rolling. Figure 2As shown, the swing heating furnace is arranged on the conveying equipment of the continuous casting machine. The swing heating furnace includes a heating section and a swing section. After the continuous casting slab enters the heating section through the conveying equipment and is heated to a preset temperature, it is conveyed to the hot rolling along the swing section. The first swing heating furnace and the second swing heating furnace can be arranged in parallel or side by side. The swing section of the first swing heating furnace / the second swing heating furnace can change the conveying path of the steel billet by rotating, and the steel billet can be conveyed to the hot rolling connected to the first swing heating furnace for alternating hot rolling. The uneven wear of the local roller can be reduced, thereby reducing the convexity after rolling.

[0045] In some embodiments, the physicochemical data of the electrical steel and the non-electrical steel include steel slab composition. In order to reduce the crown of the electrical steel after rolling, the rolling parameters need to be adjusted to match the physicochemical data of the electrical steel and the non-electrical steel.

[0046] In some embodiments, in the swing heating furnace, the heating temperature of the electrical steel ingot is 1100-1160° C., and the furnace discharge temperature is 1020-1080° C. The temperature of the electrical steel ingot will affect the temperature of the internal impurities, which will in turn affect the rolling parameters (such as rolling force, working roll speed, etc.) and the amount of cooling water.

[0047] In some embodiments, the self-learning model includes short-term learning and long-term learning.

[0048] In some embodiments, short-term learning includes: first inputting the physical and chemical data, rolling parameters and convexity of steel billets with different furnace numbers into the model, training the model, obtaining the functional relationship between the physical and chemical data of the steel billets, rolling parameters and convexity, and then inputting the set convexity value and the physical and chemical data of the steel billets. The model obtains the corresponding rolling parameters according to the functional relationship obtained by training, and then adjusts and implements through the basic automation system; distinguishing the slabs in the first swing heating furnace and the second swing heating furnace, and learning the data of the corresponding heating furnace respectively. Steel billets from different furnace numbers are different in composition and performance. The short-term learning model can ensure the temperature, plate shape index and threading stability, and adjust the working roll shifting strategy.

[0049] In some embodiments, long-term learning includes: first inputting the physical and chemical data, rolling parameters and convexity after rolling of billets of different steel grades into the model, training the model, obtaining the functional relationship between the physical and chemical data of the billet, rolling parameters and convexity, and then inputting the set convexity value and the physical and chemical data of the billet. The model obtains the corresponding rolling parameters according to the functional relationship obtained by training, and then adjusts and implements through the basic automation system; subdividing the physical and chemical data and rolling parameters of the billet, dividing into small intervals, and continuously optimizing the model data. Billets of different steel grades are different in composition and performance. The long-term learning model can be refined and differentiated according to steel grades and specifications, thereby improving the control accuracy of the model.

[0050] The self-learning model includes rolling force model, pass model, thickness model, width model, final rolling temperature model, laminar cooling model and plate shape control model. The rolling force model calculates the rolling force, rolling torque, rolling work and forward slip parameters required by the automation system in the production process according to the steel coil data, mechanical parameters, rolled material characteristics and the calculation type required by the process. The pass model is used to calculate the reduction amount and roll gap of each stand. The thickness model follows the principle of second flow rate and uses the basic automation system to calculate the reduction position, tension and rolling speed of each stand, and then compares it with the thickness gauge detection value to control the thickness within the tolerance range. The width model performs width reduction load distribution, pass plan pre-calculation, post-calculation, adaptation, feedforward control, feedback control and short stroke control according to the incoming width of the slab and the finishing width, and calculates and measures the natural width of the finishing rolling. The final rolling temperature model calculates the temperature drop of the hot-rolled strip in the finishing area based on the calculation data of the finishing passes, calculates the timing and water volume setting of the cooling water spray between the racks, etc., to ensure that the target temperature value after finishing rolling is achieved and the temperature consistency of the strip is guaranteed. The laminar cooling model calculates the opening mode, number of openings and opening time of the laminar cooling valve according to the temperature after finishing rolling and the curling target temperature, and makes head adjustments. And according to the actual measurement of the strip temperature, feedforward control, feedback control, post-calculation and adaptive calculation are performed. The plate shape control model calculates the CVC and bending roll force according to the target value, controls the cross-sectional shape of the strip, and controls the occurrence of various corrugated plates.

[0051] In some embodiments, in the step of refining the electrical steel molten steel and the non-electrical steel molten steel, the electrical steel molten steel is obtained by sequentially processing through a blast furnace, a KR furnace, a converter, and a RH furnace, and the non-electrical steel molten steel is obtained by sequentially processing through a blast furnace, a KR furnace, a converter, and a RH furnace. Figure 1 As shown, the blast furnace, KR, converter, RH furnace and continuous casting machine are connected in sequence. Refined molten steel can be obtained after smelting in the blast furnace, KR, converter and RH furnace. Different types of steel (one of which is non-oriented electrical steel) are cast separately through two continuous casting machines to obtain slabs.

[0052] In some embodiments, in the step of performing alternating hot rolling on the electrical steel ingot and the non-electrical steel ingot to obtain the small convex electrical steel, the alternating hot rolling is performed using a seven-stand finishing mill. Figure 3 As shown, the hot rolling mill includes a finishing mill vertical roll, a seven-stand finishing mill, an ultra-fast cooling device, a laminar cooling and a down coiler which are arranged in sequence.

[0053] On the one hand, the vertical rollers of the finishing mill can be used to remove phosphorus during the rolling process. The large vertical rollers can loosen the oxidized iron scale on the surface of the slab, and then use high-pressure water impact to achieve a good dephosphorization effect. On the other hand, it can also be used for side rolling of the slab. After side rolling of the slab, the drum shape and cracking of the edge of the rolled piece can be avoided, and the width standard of the strip can be adjusted to obtain a strip with uniform width and neat edges, thereby reducing the metal consumption coefficient.

[0054] In some embodiments, the hot rolling is followed by acid rolling, which can roll the hot-rolled substrate to a target thickness to ensure the quality of the plate shape.

[0055]

Small convex electrical steel

[0056] A small convex electrical steel is obtained by the above preparation method.

[0057] In some embodiments, the average convexity of the small-convex electrical steel is 20-21 μm. The average convexity refers to the average convexity of the electrical steel on each surface.

[0058] In some embodiments, among the electrical steels with small convexity, the proportion of convexity ≤25 μm is 82%-93%, and the proportion of convexity ≤30 μm is 95%-100%. It can be seen that the convexity of the electrical steel provided in this application is very small on each surface.

[0059]

Application of small convex electrical steel in motor electronics

[0060] An application of small-convex electrical steel in motors and electronics, wherein the small-convex electrical steel is selected from the small-convex electrical steel obtained by the above-mentioned preparation method or the above-mentioned small-convex electrical steel.

[0061] Example

[0062] Train short-term learning models and long-term learning models.

[0063] The target convexity value and the target specifications of electrical steel and other steel grades (such as thickness and composition) are input into the secondary process control system. The basic automation system receives the set process parameter information fed back by the self-learning model and controls the equipment according to these set data.

[0064] Then press Figure 1 As shown in the figure, ore, coke and flux are added into the furnace from the top of the blast furnace in a certain proportion, and refined molten steel is obtained through smelting in the blast furnace, KR furnace, converter and RH furnace in sequence. The refined molten steel is then transported to the continuous casting machine through a steel ladle to obtain slabs of different steel grades. Figure 2 The swing heating furnace shown heats slabs of different steel grades and then transfers them alternately to the hot rolling mill. Figure 3The hot rolling process shown in the figure is processed by the finishing mill vertical roller, seven-stand finishing mill, ultra-fast cooling device, laminar cooling and down coiler to obtain small crown electrical steel and other steel grades of different furnace numbers. The specific data are shown in Table 1:

[0065] Table 1

[0066]

[0067]

[0068] The non-oriented electrical steels in Table 1 were then subjected to acid rolling treatment, and the plate difference and surface quality tests were performed.

[0069] Pickling treatment: The hot rolled coil is straightened and pickled before rolling in a cold rolling mill.

[0070] The test results are shown in Table 2:

[0071] Table 2

[0072] Pickling Roll No. Tension leveling elongation The first stand pressing rate Difference between the same board, μm Surface quality A302017700 2.70% 30% 4 No tendons A302016500 2.70% 30% 4 No tendons A302016400 2.70% 30% 3 No tendons A302016300 2.70% 30% 3 No tendons A302016200 2.70% 30% 4 No tendons A302017400 2.70% 30% 3 No tendons A302017100 2.70% 30% 3 No tendons A302017500 2.70% 30% 4 No tendons A302017300 2.70% 30% 4 No tendons A302092300 2.70% 30% 6 No tendons

[0073] It can be seen from Table 1 and Table 2 that the non-oriented electrical steel obtained in the examples of the present application has a small convexity, and the surface quality after acid rolling is normal without rib defects.

[0074] Comparative Example 1

[0075] The experimental steps are the same as those in the embodiment, except that "alternative hot rolling of electrical steel and other steel grades" is changed to "only hot rolling of electrical steel" to obtain non-oriented electrical steel, which is then subjected to acid rolling treatment, and the convexity, plate difference and surface quality are tested. The results are shown in Table 3:

[0076] Table 3

[0077]

[0078] It can be seen from Table 1, Table 2 and Table 3 that alternating hot rolling can reduce the uneven wear of the local rolls, thereby reducing the convexity of the non-oriented electrical steel. After acid rolling treatment, the difference between the same plate is small.

Claims

1. A method for preparing small crown electrical steel, comprising an automatic control system and a casting and rolling device, characterized in that: The thin slab continuous casting and rolling process is adopted for production. The preparation method comprises: refining electrical steel molten steel and non-electrical steel molten steel to obtain refined electrical steel molten steel and refined non-electrical steel molten steel, wherein the refined electrical steel molten steel contains the following components in mass percentage: 0.000%≤C≤0.006%, 0.3%≤Si≤0.9%, 0.2%≤Mn≤0.5%, 0.01%≤P≤0.1%, 0.000%≤S≤0.006%, 0.2%≤Al≤0.5%, 0.0000%≤N≤0.0050% and 0.0000%≤Ti≤0.0050%, and the rest are iron and inevitable trace elements; Continuously casting the refined electrical steel molten steel and the refined non-electrical steel molten steel respectively to obtain electrical steel ingots and non-electrical steel ingots; Alternately hot-rolling the electrical steel ingot and the non-electrical steel ingot to obtain the small-crown electrical steel; The automation control system includes a basic automation system and a secondary process control system, and the secondary process control system includes a self-learning model, and the self-learning model is used to optimize rolling parameters including work roll shifting, bending roll force dynamics and rolling temperature according to the physical and chemical data of electrical steel and non-electrical steel, rolling parameters and the functional relationship of the convexity after rolling; the physical and chemical data of electrical steel and non-electrical steel include billet composition; The step of alternately hot rolling the electrical steel ingot and the non-electrical steel ingot comprises: The electrical steel ingot and the non-electrical steel ingot are placed in a first swing heating furnace and a second swing heating furnace respectively, the outlet of the first swing heating furnace is connected to hot rolling, and the electrical steel ingot or the non-electrical steel ingot is transported from the second swing heating furnace to the first swing heating furnace through the swing section of the heating furnace for alternating hot rolling; In the swing heating furnace, the heating temperature of the electrical steel ingot is 1100-1160°C, and the furnace discharge temperature is 1020-1080°C; The self-learning model includes short-term learning and long-term learning; The short-term study includes: First, the physical and chemical data, rolling parameters and convexity after rolling of steel billets with different furnace numbers are input into the model, and the model is trained to obtain the functional relationship between the physical and chemical data of the steel billets, the rolling parameters and the convexity. Then, the set convexity value and the physical and chemical data of the steel billets are input, and the model obtains the corresponding rolling parameters according to the functional relationship obtained by training, and then the basic automation system is used to adjust and implement; the steel billets in the first swing heating furnace and the second swing heating furnace are distinguished, and the data of the corresponding heating furnaces are learned for each; The long-term learning includes: First, the physicochemical data, rolling parameters and convexity after rolling of steel billets of different steel grades are input into the model, and the model is trained to obtain the functional relationship between the physicochemical data of the steel billet, the rolling parameters and the convexity. Then, the set convexity value and the physicochemical data of the steel billet are input, and the model derives the corresponding rolling parameters according to the functional relationship obtained through training, and then adjusts and implements them through the basic automation system; the physicochemical data and rolling parameters of the steel billet are subdivided, divided into small intervals, and the model data is continuously optimized.

2. The preparation method according to claim 1, characterized in that: In the step of refining electrical steel molten steel and non-electrical steel molten steel, the electrical steel molten steel is obtained by sequentially processing through a blast furnace, KR, a converter and a RH furnace, and the non-electrical steel molten steel is obtained by sequentially processing through a blast furnace, KR, a converter and a RH furnace.

3. The preparation method according to claim 1, characterized in that: In the step of performing alternating hot rolling on the electrical steel ingot and the non-electrical steel ingot to obtain the small-convex electrical steel, the alternating hot rolling is performed using a seven-stand finishing mill.

4. The preparation method according to claim 1, characterized in that: After the step of alternately hot-rolling the electrical steel ingot and the non-electrical steel ingot to obtain the small-convex electrical steel, the method further includes the steps of layer cooling treatment and coiling treatment, wherein the coiling temperature is 600-700°C.

5. The preparation method according to claim 1, characterized in that: The alternating hot rolling also includes pickling.

6. A small crown electrical steel, characterized in that: The method is obtained by the preparation method described in any one of claims 1 to 5.

7. The small crown electrical steel according to claim 6, characterized in that: In the small-convex electrical steel, the average convexity is 20-21 μm.

8. The small crown electrical steel according to claim 6, characterized in that: Among the small-convex electrical steels, those with a convexity of ≤25 μm account for 82%-93%, and those with a convexity of ≤30 μm account for 95%-100%.

9. Application of small convexity electrical steel in motor electronics, characterized in that: The small crown electrical steel is selected from the small crown electrical steel according to any one of claims 6 to 8.