An antimony-based multi-element alloy material and its application in lithium-ion batteries

Through the composite of antimony-based multi-alloy material and carbon aerogel, the combination of transition metals, non-metals and rare earth elements is used to form nano-level alloy materials, which solves the problem of volume expansion of tin and antimony metals in lithium-ion batteries and improves the battery cycling stability and electrochemical properties.

CN117790765BActive Publication Date: 2024-11-26HUNAN LOUDI HUAXING ANTIMONY IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311785089.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-26
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

Tin and antimony metals cause severe volume expansion during the charging and discharging of lithium-ion batteries, resulting in unstable negative electrode structure, powdering and collapse of materials, affecting the cyclic stability and rate performance of the electrode.

Method used

Antimony-based multi-alloy material is used to form nano-level alloy materials through the combination of transition metal elements, non-metal elements and rare earth elements, and composite them with carbon aerogels to buffer volume changes through covalent bonds and three-dimensional network structure to improve the material cycling performance.

Benefits of technology

It effectively reduces the deformation stress during the deintercalation of lithium/sodium, extends the life of lithium batteries, improves electrochemical performance and cyclic stability, and enhances the stability of the material and lithium storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117790765B_ABST
    Figure CN117790765B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium ion batteries, in particular to an antimony-based multi-element alloy material and application thereof in a lithium ion battery. The antimony-based multi-element alloy material comprises the following elements in weight percentage: A 7.5-15%, B 1-3%, C 0.01-0.1%, Sn 10-20%, and the balance Sb; wherein A is a transition metal element; B is a non-metallic element; and C is a rare earth element. The lithium battery prepared by the antimony-based multi-element alloy material has high discharge specific capacity and cycle stability, and after being compounded with carbon aerogel, the electrochemical performance is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, in particular to an antimony-based multi-element alloy material and application thereof in lithium ion batteries. Background Art

[0002] Lithium-ion battery is a high energy density power source, and its outstanding advantages are high operating voltage, high energy density, long cycle life, no environmental pollution, etc. Since the negative electrode material has a significant impact on the capacity and cycle life of lithium-ion batteries, it has become the research focus of the battery industry around the world.

[0003] Graphite or modified carbon materials are traditional negative electrode materials and have been commercialized. However, since only one lithium can be embedded in every six carbon atoms, its theoretical capacity is low. At the same time, the lithium deintercalation potential of carbon materials is close to the lithium precipitation potential, which affects the safety of the battery during the charge and discharge process. Therefore, many researchers have turned their attention to non-carbon materials.

[0004] Among non-carbon materials, antimony and tin have attracted widespread attention due to their high theoretical capacity, small electrode polarization and moderate operating voltage. However, tin and antimony metals will produce severe volume expansion during the charging and discharging process, and the negative electrode structure cannot remain stable after deintercalation, resulting in material pulverization and collapse, and eventually material rupture, resulting in poor electrode cycle stability and rate performance. Therefore, the development of alloy materials with high specific capacity and high cycle stability is of great significance for expanding the commercial application scenarios of lithium-ion batteries. Summary of the invention

[0005] Purpose of the invention: In view of the above technical problems, the present invention proposes an antimony-based multi-element alloy material and its application in lithium-ion batteries.

[0006] The technical solutions adopted are as follows:

[0007] An antimony-based multi-element alloy material, comprising the following elements by weight percentage:

[0008] A 7.5-15%, B 1-3%, C 0.01-0.1%, Sn 10-20%, the balance is Sb;

[0009] Wherein, A is a transition metal element;

[0010] B is a non-metallic element;

[0011] C is a rare earth element.

[0012] Furthermore, A is any one or more combinations of Fe, Co, Ni, Cu and Zn.

[0013] Furthermore, A is Fe, Co and Ni, and the weight ratio of Fe, Co and Ni is 1-5:1-5:1-5.

[0014] Furthermore, B is any one or more combinations of Si, P, and S.

[0015] Further, B is P.

[0016] Furthermore, C is any one or more combinations of La, Ce, Sm, and Dy.

[0017] Furthermore, C is Ce.

[0018] The present invention also provides an application of the antimony-based multi-element alloy material in a lithium-ion battery.

[0019] Furthermore, the negative electrode material of the lithium-ion battery includes a combination of the antimony-based multi-element alloy material and carbon aerogel.

[0020] Furthermore, the preparation method of the composition is as follows:

[0021] Weigh each raw material in proportion, ball-mill them uniformly under the protection of inert gas, press the obtained mixture into a cylinder, use a six-sided top press to synthesize the antimony-based multi-element alloy material at a pressure and temperature of 4-6GP and 1200-1400°C, anneal it at 700-900°C, crush it and ball-mill it again to obtain a nano-level alloy powder, disperse the alloy powder in anhydrous ethanol to obtain a dispersion, add formaldehyde, resorcinol and sodium carbonate into water, blend the obtained solution with the dispersion, heat to 50-70°C, seal and react for 60-120h, place the obtained wet gel for aging in tert-butanol for solvent replacement for 5-10d, replace fresh tert-butanol every day, and finally freeze-dry and carbonize at 850-950°C under the protection of inert gas.

[0022] Beneficial effects of the present invention:

[0023] The present invention provides an antimony-based multi-element alloy material, the nanometer-level size of which can reduce the deformation stress generated by the active material in the process of lithium / sodium intercalation and deintercalation to a certain extent, improve the reaction efficiency, and can effectively buffer the volume change in the cycle process, thereby inhibiting pulverization and agglomeration, wherein the transition metal element is an inactive substance, and begins to agglomerate to form a free state in the process of lithium ion intercalation and deintercalation, slowing down the drastic volume shrinkage during lithium intercalation and deintercalation, playing a role in stabilizing the skeleton and improving its cycle performance, non-metallic elements can form compounds with transition metal elements and rare earth elements, and due to their high degree of electron delocalization and low oxidation state of metal elements, they can form stronger covalent bonds, and thus have better cycle performance and stability, and the introduction of appropriate non-metallic elements can prolong the life of lithium batteries, and rare earth elements have A certain solid solubility can cause micro-alloying in transition metal elements with small solid solubility. At the same time, the segregation of rare earth elements at the grain boundaries inhibits the growth of grains, strengthens the grain boundaries, improves the stability of the alloy material during the charge and discharge process, and improves its cycle performance as a negative electrode material. Carbon aerogel not only has good conductivity, but more importantly, its unique three-dimensional network structure can give full play to the lithium storage performance of the alloy material, improve the agglomeration phenomenon of the alloy material, buffer the volume expansion during the charge and discharge process, and is conducive to better contact between the active substance and the electrolyte, thereby improving the cycle performance. After testing, the lithium battery prepared by the antimony-based multi-element alloy material in the present invention has a higher discharge specific capacity and cycle stability, and after being compounded with the carbon aerogel, the electrochemical performance is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the TEM image of the antimony-based multi-element alloy material prepared in Example 1. DETAILED DESCRIPTION

[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0026] Embodiment 1:

[0027] An antimony-based multi-element alloy material, comprising the following elements by weight percentage:

[0028] Fe 6.5%, Co 6.5%, Ni 1.5%, P 2.5%, Ce 0.05%, Sn 16%, balance Sb;

[0029] The preparation method is as follows:

[0030] Fe powder, Co powder, Ni powder, P powder, Ce powder, Sn powder and Sb powder are weighed according to the above weight proportion, and mechanically ball-milled in a planetary ball mill for 10 hours under argon protection to make the mixture uniform. After ball milling, the obtained mixture is dried, and then placed in a mold and pressed into a cylinder under a pressure of 5 MPa, and then a six-sided top press is used to keep the temperature at 1300°C for 30 minutes at a pressure of 6GP to synthesize the antimony-based multi-element alloy material. The material is taken out, annealed at 800°C for 10 hours, crushed, and again mechanically ball-milled at a speed of 200 r / min for 10 hours in a planetary ball mill under argon protection and dried to obtain an alloy powder with a particle size of 10-200 nm.

[0031] Embodiment 2:

[0032] An antimony-based multi-element alloy material, comprising the following elements by weight percentage:

[0033] Fe 6.5%, Co 6.5%, Ni 1.5%, P 3%, Ce 0.1%, Sn 20%, balance Sb;

[0034] The preparation method is as follows:

[0035] Fe powder, Co powder, Ni powder, P powder, Ce powder, Sn powder and Sb powder are weighed according to the above weight proportion, and mechanically ball-milled in a planetary ball mill for 10 hours under argon protection to make the mixture uniform. After ball milling, the obtained mixture is dried, and then placed in a mold and pressed into a cylinder under a pressure of 5 MPa, and then a six-sided top press is used to keep the temperature at 1300°C for 30 minutes at a pressure of 6GP to synthesize the antimony-based multi-element alloy material. The material is taken out, annealed at 800°C for 10 hours, crushed, and again mechanically ball-milled at a speed of 200 r / min for 10 hours in a planetary ball mill under argon protection and dried to obtain an alloy powder with a particle size of 10-200 nm.

[0036] Embodiment 3:

[0037] An antimony-based multi-element alloy material, comprising the following elements by weight percentage:

[0038] Fe 6.5%, Co 6.5%, Ni 1.5%, P 1%, Ce 0.01%, Sn 10%, balance Sb;

[0039] The preparation method is as follows:

[0040] Fe powder, Co powder, Ni powder, P powder, Ce powder, Sn powder and Sb powder are weighed according to the above weight proportion, and mechanically ball-milled in a planetary ball mill for 10 hours under argon protection to make the mixture uniform. After ball milling, the obtained mixture is dried, and then placed in a mold and pressed into a cylinder under a pressure of 5 MPa, and then a six-sided top press is used to keep the temperature at 1300°C for 30 minutes at a pressure of 6GP to synthesize the antimony-based multi-element alloy material. The material is taken out, annealed at 800°C for 10 hours, crushed, and again mechanically ball-milled at a speed of 200 r / min for 10 hours in a planetary ball mill under argon protection and dried to obtain an alloy powder with a particle size of 10-200 nm.

[0041] Embodiment 4:

[0042] A method for preparing a composition:

[0043] 1 g of the alloy powder prepared in Example 1 and 0.1 g of PVP were added to 20 ml of anhydrous ethanol and ultrasonically oscillated for 30 min to obtain a dispersion, 60 g of formaldehyde, 110 g of resorcinol and 1 g of sodium carbonate were added to 250 ml of deionized water and mixed to obtain a solution, the dispersion was added to the solution and stirred and blended, heated to 70°C and sealed for reaction for 120 h, and the wet gel was aged for 24 h. The wet gel was placed in tert-butanol for solvent replacement for 5 days, during which fresh tert-butanol was replaced every day, and finally freeze-dried at low temperature, heated to 950°C at a rate of 15°C / min under argon protection and carbonized for 2 h.

[0044] Embodiment 5:

[0045] A method for preparing a composition:

[0046] 1 g of the alloy powder prepared in Example 2 and 0.1 g of PVP were added to 20 ml of anhydrous ethanol and ultrasonically oscillated for 30 min to obtain a dispersion, 60 g of formaldehyde, 110 g of resorcinol and 1 g of sodium carbonate were added to 250 ml of deionized water and mixed to obtain a solution, the dispersion was added to the solution and stirred, heated to 70°C and sealed for reaction for 120 h, and the wet gel was aged for 24 h. The wet gel was placed in tert-butanol for solvent replacement for 5 days, during which fresh tert-butanol was replaced every day, and finally freeze-dried at low temperature, heated to 950°C at a rate of 15°C / min under argon protection and carbonized for 2 h.

[0047] Embodiment 6:

[0048] A method for preparing a composition:

[0049] 1 g of the alloy powder prepared in Example 3 and 0.1 g of PVP were added to 20 ml of anhydrous ethanol and ultrasonically oscillated for 30 min to obtain a dispersion, 60 g of formaldehyde, 110 g of resorcinol and 1 g of sodium carbonate were added to 250 ml of deionized water and mixed to obtain a solution, the dispersion was added to the solution and stirred, heated to 70°C and sealed for reaction for 120 h, and the wet gel was aged for 24 h. The wet gel was placed in tert-butanol for solvent replacement for 5 days, during which fresh tert-butanol was replaced every day, and finally freeze-dried at low temperature, heated to 950°C at a rate of 15°C / min under argon protection and carbonized for 2 h.

[0050] Performance Testing:

[0051] The electrochemical performance test was carried out using a CR2032 button cell. The CR2032 button cell was assembled in a glove box. The active material, conductive carbon black, and binder PVDF (HSV900) prepared in Examples 1-6 were mixed and ground in a mass ratio of 80:10:10, and then evenly coated on a copper foil. The mixture was vacuum dried in a vacuum drying oven at 120°C for 12 hours. A pure lithium sheet was used as a counter electrode, Celgard2300 was used as a diaphragm material, and an electrolyte solution of 1M LiPF6 in ethylene carbonate and dimethyl ethylene carbonate (volume ratio of 1:1) was used. A LAND CT2001A battery tester was used at 25°C and 1000 mA / g was used to perform 500 charge and discharge cycles between 0.01-2.5V. The test results are shown in Table 1.

[0052] Table 1:

[0053]

[0054] It can be seen from Table 1 that the lithium battery prepared by the antimony-based multi-element alloy material in the present invention has a higher discharge specific capacity and cycle stability, and the electrochemical performance is further improved after being compounded with the carbon aerogel.

[0055] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An antimony-based multi-element alloy material, characterized in that: The following elements are included in weight percentage: A 7.5-15%, B 1-3%, C 0.01-0.1%, Sn 10-20%, the balance is Sb; Wherein, A is Fe, Co and Ni, and the weight ratio of Fe, Co and Ni is 1-5:1-5:1-5; B is P; C is Ce; Application of the antimony-based multi-element alloy material in a lithium-ion battery, wherein the negative electrode material of the lithium-ion battery comprises a combination of the antimony-based multi-element alloy material and carbon aerogel; The preparation method of the composition is as follows: Weigh each raw material in proportion, ball-mill them uniformly under the protection of inert gas, press the obtained mixture into a cylinder, use a six-sided top press to synthesize the antimony-based multi-element alloy material at a pressure and temperature of 4-6GP and 1200-1400°C, anneal it at 700-900°C, crush it and ball-mill it again to obtain a nano-level alloy powder, disperse the alloy powder in anhydrous ethanol to obtain a dispersion, add formaldehyde, resorcinol and sodium carbonate into water, blend the obtained solution with the dispersion, heat to 50-70°C, seal and react for 60-120h, place the obtained wet gel for aging in tert-butanol for solvent replacement for 5-10d, replace fresh tert-butanol every day, and finally freeze-dry and carbonize at 850-950°C under the protection of inert gas.