A method for preparing a fiber composite shell backing coating

By pretreating the steel fibers and mixing them with silica sol and refractory powder, the problem of steel fibers being easy to entangle and difficult to disperse in the shell backing coating was solved, thus improving the wet strength of the shell.

CN117802778BActive Publication Date: 2026-11-17INNER MONGOLIA UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310604137.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2026-11-17
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

During the preparation of the shell backing coating, steel fibers are prone to entanglement and are difficult to disperse, which weakens the shell's wet strength enhancement effect.

Method used

By pretreating steel fibers, including immersing them in a sodium hydroxide solution and coating them with a carboxylic acid-based polyurethane film, and then mixing them with silica sol and refractory powder under ultrasonic conditions, a fiber composite shell backing coating is formed.

Benefits of technology

It improves the dispersibility of steel fibers in coatings, increases the wet strength of the shell, and avoids the strength reduction caused by fiber agglomeration.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing a fiber-reinforced composite shell backing coating, comprising the following steps: Step A: Pre-treating the fibers to obtain pre-treated fibers; Step B: Pouring the pre-treated fibers into silica sol and stirring under ultrasonic conditions to obtain a silica sol dispersion; Step C: Adding refractory powder to the silica sol dispersion and continuing to stir under ultrasonic conditions to obtain the fiber-reinforced composite shell backing coating. The fiber-reinforced composite shell backing coating prepared by the method of this invention exhibits good fiber dispersibility, thereby avoiding the problem of weakened wet strength enhancement effect on the shell due to fiber agglomeration. The shell prepared using the fiber-reinforced composite shell backing coating of this invention shows a significant improvement in wet strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of shell preparation technology. Specifically, it relates to a method for preparing a back coating for a fiber composite shell. Background Technology

[0002] In recent years, investment casting has been widely used in aerospace, aviation, automotive, and weaponry fields due to its advantages such as precise casting dimensions, smooth surface, and no limitation on alloy materials, making it suitable for manufacturing complex-shaped castings. In actual production, the quality of the mold shell is a key factor affecting the quality of the casting. The mold shell generally consists of a face layer, a transition layer, and a back layer. Different shell layers have different performance requirements. The back layer does not contact the molten metal and is mainly used to ensure that the mold shell has good strength and resistance to deformation. The mold shell is generally composed of refractory materials, binders, and additives, and is prepared through processes such as coating, sand application, drying, hardening, dewaxing, and firing. Commonly used binders include water glass, silica sol, and ethyl silicate. Among them, silica sol has become the most widely used binder due to its good high-temperature firing strength.

[0003] For shell backing layers, shells prepared using silica sol-based shell backing coatings typically suffer from low wet strength (room temperature strength). Therefore, increasing the shell thickness is used to improve the wet strength of the silica sol shell. However, increasing the shell thickness reduces its thermal conductivity, making heat dissipation difficult and leading to coarse casting structure and decreased performance. Therefore, steel fibers are added as a reinforcing phase to the shell backing coating to improve both the shell's strength and its thermal conductivity.

[0004] Because the steel fibers are produced using a "bundled drawing method," the fibers are cylindrical in shape, but their surfaces have irregular grooves due to compression from other fibers. Furthermore, to prevent fiber adhesion during the drawing process, an organic solvent is applied to the surface. Therefore, the steel fibers are not easily wetted by silica sol, and the grooves create significant surface friction, making the fibers prone to entanglement and difficult to disperse. This severely weakens the fiber's ability to enhance the wet strength of the shell backing layer. Summary of the Invention

[0005] Therefore, the technical problem to be solved by the present invention is to provide a method for preparing a fiber composite shell backing coating, so as to solve the problem that the shell wet strength enhancement effect is weakened due to the easy entanglement and difficulty in dispersion of fibers during the preparation of the shell backing coating.

[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0007] A method for preparing a fiber composite shell backing coating includes the following steps:

[0008] Step A: Clean the fibers to obtain pretreated fibers;

[0009] Step B: Pour the pretreated fibers into the silica sol and stir under ultrasonic conditions to obtain a silica sol dispersion;

[0010] Step C: Add refractory powder to the silica sol dispersion and continue stirring under ultrasonic conditions to obtain a fiber composite shell backing coating.

[0011] In the preparation method of the above-mentioned fiber composite shell back coating, in step B, the amount of pretreated fiber added is 0.10-0.15 wt% of the silica sol mass; the silica content in the silica sol is 20-30 wt%; the pH of the silica sol is 9-10; the ultrasonic frequency is 28 kHz; the ultrasonic power is 600-1000 W; and the ultrasonic stirring time is 0.5-1 h.

[0012] In the preparation method of the above-mentioned fiber composite shell backing coating, the mass ratio of silica sol dispersion to refractory powder in step C is 1:1-1.5.

[0013] In the preparation method of the above-mentioned fiber composite shell backing coating, the refractory powder in step C is composed of 80-100 parts by weight of mullite powder, 15-20 parts by weight of fused silica powder and 5-15 parts by weight of zircon powder; the refractory powder passes through a 200-mesh sieve.

[0014] In the preparation method of the above-mentioned fiber composite shell backing coating, in addition to cleaning, step A also includes the following pretreatment step:

[0015] Step (A-1): Soak the steel fiber in sodium hydroxide solution. After soaking, wash the steel fiber with water until the washing solution is neutral. Dry the washed steel fiber.

[0016] Step (A-2): Add the dried steel fibers to the waterborne polyurethane and stir to completely submerge the surface of the steel fibers in the waterborne polyurethane, thus obtaining impregnation system A;

[0017] Step (A-3): Add ammonium zirconium carbonate solution to impregnation system A under stirring and stir until well mixed to obtain impregnation system B;

[0018] Step (A-4): Remove the steel fibers from the impregnation system B, drain them, and dry them in a drying oven to obtain pretreated steel fibers.

[0019] In the preparation method of the above-mentioned fiber composite shell back coating, in step (A-1), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 10-20 wt%, and the soaking time is 30-60 min; the length of the steel fiber is 2-5 mm, and the diameter is 5-10 μm.

[0020] In the preparation method of the above-mentioned fiber composite shell backing coating, in step (A-2), the waterborne polyurethane is a carboxylic acid polyurethane resin dispersion or a carboxylic acid polyurethane resin emulsion; the mass fraction of carboxylic acid polyurethane resin in the waterborne polyurethane is 50-60 wt%; and the mass fraction of carboxyl groups in the carboxylic acid polyurethane resin is 3-5 wt%.

[0021] In the preparation method of the above-mentioned fiber composite shell back coating, in step (A-2), the mass ratio of steel fiber to waterborne polyurethane is 1:1-2; in step (A-3), the volume ratio of the added zirconium ammonium carbonate solution to the waterborne polyurethane in step (A-2) is 1:40-60.

[0022] In the preparation method of the above-mentioned fiber composite shell back coating, in step (A-3), the mass fraction of zirconium carbonate in the zirconium carbonate solution is 10-15 wt%.

[0023] In the preparation method of the above-mentioned fiber composite shell backing coating, in step (A-4), the drying temperature is 40-60℃ and the drying time is 2-3h.

[0024] The technical solution of the present invention achieves the following beneficial technical effects:

[0025] 1. The fiber composite shell backing coating prepared by the method of the present invention has good fiber dispersibility, which can avoid the problem of weakened fiber enhancement effect on the wet strength of the shell due to fiber agglomeration in the coating. Using the fiber composite shell backing coating of the present invention to prepare the shell can significantly improve the wet strength of the shell.

[0026] 2. This invention improves the hydrophilicity of steel fibers by pretreating them, making them easier to disperse in silica sol. Coating the steel fibers with a carboxylic acid-based polyurethane film not only effectively enhances their hydrophilicity but also fills irregular grooves on the fiber surface caused by compression from other fibers during production. This results in a smoother, flatter surface, reduced friction, and improved fiber agglomeration.

[0027] 3. In the pretreatment of steel fibers, this invention selects carboxylic acid polyurethane resin emulsion with a carboxyl group mass fraction of 3-5 wt% and ammonium zirconium carbonate as raw materials to carry out a film-forming reaction on the surface of steel fibers. This can obtain a coating with better hydrophilicity on the surface of steel fibers. At the same time, the formation of the coating effectively increases the surface area of ​​steel fibers and reduces the density of steel fibers to a certain extent. This effectively prevents the phenomenon that steel fibers are easy to sink during stirring due to their relatively high density, and allows them to be completely dispersed in a shorter time under ultrasonic conditions.

[0028] 4. This invention selects a mixture of mullite powder, fused silica powder, and zircon powder as the refractory powder in the backing coating. Compared with using a single mullite powder or a mixture of mullite powder and fused silica powder as the refractory powder in the backing coating, this method can further improve the dispersibility of steel fibers in the backing coating and the wet strength of the shell. This may be because: when 3-5 wt% of carboxylic acid polyurethane resin and ammonium zirconium carbonate form a coating on the surface of the steel fibers, the anionic hydroxylated zirconium polymer in the coating can form a stronger bond with zirconium silicate, the main component of zirconium powder, under the ultrasonic conditions of this invention. This makes it easier for the steel fibers to disperse in the backing coating and allows the steel fibers in the final shell to be more tightly bonded to the refractory powder, thereby effectively improving the effect of steel fibers on enhancing the wet strength of the shell. Detailed Implementation

[0029] Example 1

[0030] The preparation method of the fiber composite shell backing coating in this embodiment includes the following steps:

[0031] Step A: Clean the steel fibers to obtain pretreated steel fibers. The cleaning method for steel fibers is as follows: immerse steel fibers with a length of 5 mm and a diameter of 10 μm in a 10 wt% sodium hydroxide solution for 60 min. After immersion, wash the steel fibers with clean water until the washing solution is neutral. Dry the washed steel fibers to obtain pretreated steel fibers.

[0032] Step B: Pour the pretreated steel fibers into the silica sol. The amount of pretreated steel fibers added is 0.15 wt% of the silica sol mass. The silica content in the silica sol is 30 wt%, and the pH of the silica sol is 9. The silica sol is then ultrasonically stirred for 1 h under ultrasonic conditions of 28 kHz and 800 W to obtain a silica sol dispersion.

[0033] Step C: Add refractory powder to the silica sol dispersion. The mass ratio of silica sol dispersion to refractory powder is 1:1.2. The refractory powder is mullite powder that has passed through a 200-mesh sieve. Continue ultrasonic stirring for 1 hour under ultrasonic conditions of 28kHz ultrasonic frequency and 800W ultrasonic power to obtain fiber composite shell backing coating.

[0034] Example 2

[0035] The preparation method of the fiber composite shell backing coating in this embodiment includes the following steps:

[0036] Step A: Clean the steel fibers to obtain pretreated steel fibers. The cleaning method for steel fibers is as follows: immerse steel fibers with a length of 2 mm and a diameter of 10 μm in a 20 wt% sodium hydroxide solution for 50 min. After immersion, wash the steel fibers with clean water until the washing solution is neutral. Dry the washed steel fibers to obtain pretreated steel fibers.

[0037] Step B: Pour the pretreated steel fibers into the silica sol. The amount of pretreated steel fibers added is 0.10 wt% of the silica sol mass. The silica content in the silica sol is 25 wt%, and the pH of the silica sol is 10. The silica sol is then ultrasonically stirred for 1 hour under ultrasonic conditions of 28 kHz and 800 W to obtain a silica sol dispersion.

[0038] Step C: Add refractory powder to the silica sol dispersion, with a mass ratio of silica sol dispersion to refractory powder of 1:1; the refractory powder is composed of 90 parts by weight of mullite powder, 20 parts by weight of fused silica powder and 15 parts by weight of zircon powder, and passes through a 200-mesh sieve; continue ultrasonic stirring for 1 hour under ultrasonic conditions of 28 kHz ultrasonic frequency and 800 W ultrasonic power to obtain fiber composite shell backing coating.

[0039] Example 3

[0040] The preparation method of the fiber composite shell backing coating in this embodiment includes the following steps:

[0041] Step A: Pre-treat the steel fibers to obtain pre-treated steel fibers;

[0042] The method for steel fiber pretreatment includes the following steps:

[0043] Step (A-1): Immerse steel fibers with a length of 3 mm and a diameter of 10 μm in a 20 wt% sodium hydroxide solution for 30 min. After immersion, wash the steel fibers with water until the washing solution is neutral. Then dry the washed steel fibers.

[0044] Step (A-2): Add the dried steel fibers to the waterborne polyurethane and stir until the surface of the steel fibers is completely submerged in the waterborne polyurethane, to obtain impregnation system A; the waterborne polyurethane is a carboxylic acid type polyurethane resin emulsion; the mass fraction of carboxylic acid type polyurethane resin in the waterborne polyurethane is 50 wt%; the mass fraction of carboxyl groups in the carboxylic acid type polyurethane resin is 5 wt%; the mass ratio of steel fibers to waterborne polyurethane is 1:2.

[0045] Step (A-3): Add zirconium ammonium carbonate solution to impregnation system A under stirring and stir to obtain impregnation system B; the mass fraction of zirconium ammonium carbonate in the zirconium ammonium carbonate solution is 10wt%; the volume ratio of the added zirconium ammonium carbonate solution to the waterborne polyurethane is 1:60.

[0046] Step (A-4): Remove the steel fibers from the impregnation system B, drain them, and place them in a drying oven at 60°C for 2 hours to obtain pretreated steel fibers.

[0047] Step B: Pour the pretreated steel fibers into the silica sol. The amount of pretreated steel fibers added is 0.10 wt% of the silica sol mass. The silica content in the silica sol is 20 wt%, and the pH of the silica sol is 10. The silica sol is then ultrasonically stirred for 0.5 h at an ultrasonic frequency of 28 kHz and an ultrasonic power of 800 W to obtain a silica sol dispersion.

[0048] Step C: Add refractory powder to the silica sol dispersion. The mass ratio of silica sol dispersion to refractory powder is 1:1.5. The refractory powder is composed of 100 parts by weight of mullite powder, 15 parts by weight of fused silica powder and 5 parts by weight of zircon powder, and is passed through a 200-mesh sieve. Continue ultrasonic stirring for 0.5 hours under ultrasonic conditions of 28 kHz ultrasonic frequency and 800 W ultrasonic power to obtain fiber composite shell backing coating.

[0049] Example 4

[0050] The preparation method of the fiber composite shell backing coating in this embodiment includes the following steps:

[0051] Step A: Pre-treat the steel fibers to obtain pre-treated steel fibers;

[0052] The method for steel fiber pretreatment includes the following steps:

[0053] Step (A-1): Soak steel fibers with a length of 5 mm and a diameter of 5 μm in a 15 wt% sodium hydroxide solution for 40 min. After soaking, wash the steel fibers with water until the washing solution is neutral. Dry the washed steel fibers.

[0054] Step (A-2): Add the dried steel fibers to the waterborne polyurethane and stir until the surface of the steel fibers is completely submerged in the waterborne polyurethane, to obtain impregnation system A; the waterborne polyurethane is a carboxylic acid type polyurethane resin emulsion; the mass fraction of carboxylic acid type polyurethane resin in the waterborne polyurethane is 60 wt%; the mass fraction of carboxyl groups in the carboxylic acid type polyurethane resin is 3 wt%; the mass ratio of steel fibers to waterborne polyurethane is 1:1.

[0055] Step (A-3): Add zirconium ammonium carbonate solution to impregnation system A under stirring and stir to obtain impregnation system B; the mass fraction of zirconium ammonium carbonate in the zirconium ammonium carbonate solution is 15wt%; the volume ratio of the added zirconium ammonium carbonate solution to the waterborne polyurethane is 1:40.

[0056] Step (A-4): Remove the steel fibers from the impregnation system B, drain them, and place them in a drying oven at 40°C for 3 hours to obtain pretreated steel fibers.

[0057] Step B: Pour the pretreated steel fibers into the silica sol. The amount of pretreated steel fibers added is 0.10 wt% of the silica sol mass. The silica content in the silica sol is 25 wt%, and the pH of the silica sol is 9.5. The silica sol is then ultrasonically stirred for 0.5 h at an ultrasonic frequency of 28 kHz and an ultrasonic power of 800 W to obtain a silica sol dispersion.

[0058] Step C: Add refractory powder to the silica sol dispersion. The mass ratio of silica sol dispersion to refractory powder is 1:1.5. The refractory powder is composed of 100 parts by weight of mullite powder and 20 parts by weight of fused silica powder, and is passed through a 200-mesh sieve. Continue ultrasonic stirring for 0.6 hours under ultrasonic conditions of 28 kHz ultrasonic frequency and 800 W ultrasonic power to obtain fiber composite shell backing coating.

[0059] Comparative Example

[0060] The preparation method of this comparative fiber composite shell backing coating includes the following steps:

[0061] Step A: Pre-treat the steel fibers to obtain pre-treated steel fibers;

[0062] The method for steel fiber pretreatment includes the following steps:

[0063] Step (A-1): Immerse steel fibers with a length of 5 mm and a diameter of 15 μm in a 20 wt% sodium hydroxide solution for 35 min. After immersion, wash the steel fibers with water until the washing solution is neutral. Then dry the washed steel fibers.

[0064] Step (A-2): Add the dried steel fibers to the waterborne polyurethane and stir until the surface of the steel fibers is completely submerged in the waterborne polyurethane, to obtain impregnation system A; the waterborne polyurethane is a carboxylic acid type polyurethane resin emulsion; the mass fraction of carboxylic acid type polyurethane resin in the waterborne polyurethane is 45 wt%; the mass fraction of carboxyl groups in the carboxylic acid type polyurethane resin is 4 wt%; the mass ratio of steel fibers to waterborne polyurethane is 1:2.

[0065] Step (A-3): Add zirconium ammonium carbonate solution to impregnation system A under stirring and stir to obtain impregnation system B; the mass fraction of zirconium ammonium carbonate in the zirconium ammonium carbonate solution is 15wt%; the volume ratio of the added zirconium ammonium carbonate solution to the waterborne polyurethane is 1:30.

[0066] Step (A-4): Remove the steel fibers from the impregnation system B, drain them, and place them in a drying oven at 65°C for 1 hour to obtain pretreated steel fibers.

[0067] Step B: Pour the pretreated steel fibers into the silica sol. The amount of pretreated steel fibers added is 0.10 wt% of the silica sol mass. The silica content in the silica sol is 25 wt%, and the pH of the silica sol is 10. Stir mechanically for 5 hours to obtain a silica sol dispersion.

[0068] Step C: Add refractory powder to the silica sol dispersion. The mass ratio of silica sol dispersion to refractory powder is 1:1.5. The refractory powder is composed of 100 parts by weight of mullite powder, 15 parts by weight of fused silica powder and 5 parts by weight of zircon powder, and is passed through a 200-mesh sieve. Continue mechanical stirring for 5 hours to obtain a fiber composite shell backing coating.

[0069] The fiber composite shell back coatings of Examples 1 to 4 and the comparative examples were used to prepare shells, resulting in five types of shells. Each shell includes a surface layer, a transition layer, a back layer (two layers), and a sealing layer; the coatings used for the back layer and sealing layer of each shell are the same, namely the fiber composite shell back coatings prepared in the examples or comparative examples.

[0070] Preparation method of shell surface coating: Silica sol (binder) with a silica content of 25wt% is mixed with zircon powder (refractory powder) that has passed through a 325-mesh sieve at a mass ratio of 1:3, and mechanically stirred with an electric mixer for 24 hours to obtain the surface coating.

[0071] Preparation method of shell transition layer coating: Silica sol (binder) with a silica content of 25wt% is mixed with mullite powder (refractory powder) that has passed through a 200-mesh sieve at a mass ratio of 1:1.6, and mechanically stirred with an electric mixer for 24 hours to obtain the transition layer coating.

[0072] When preparing the shell, the surface layer is covered with 100 / 120 mesh zircon sand and dried for 24 hours; the transition layer is covered with 30 / 60 mesh mullite sand and dried for 24 hours; the surface layer is covered with 16 / 30 mesh mullite sand and dried for 24 hours; the sealing layer is not covered with sand and dried for 24 hours.

[0073] The wet strength of the four types of shell samples prepared was tested, and the test method referred to aviation standard: HB5352.1-2004. The average wet strength test results of the four types of shell samples (denoted as Example 1, Example 2, Example 3, Example 4 and Comparative Example) are shown in Table 1.

[0074] Table 1

[0075] Shell Example 1 Example 2 Example 3 Example 4 Comparative Example Wet strength (MPa) 3.50 3.11 4.98 4.57 4.04

[0076] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of the claims of this patent application.

Claims

1. A method for producing a fiber composite shell back layer coating, characterized by Includes the following steps: Step A: Clean the fibers to obtain pretreated fibers; Step B: Pour the pretreated fibers into the silica sol and stir under ultrasonic conditions to obtain a silica sol dispersion; Step C: Add refractory powder to the silica sol dispersion and continue stirring under ultrasonic conditions to obtain a fiber composite shell backing coating; the refractory powder in step C consists of 80-100 parts by weight of mullite powder, 15-20 parts by weight of fused silica powder and 5-15 parts by weight of zircon powder. Refractory powder passes through a 200-mesh sieve; In addition to cleaning, step A also includes the following pretreatment steps: Step (A-1): Soak the steel fiber in sodium hydroxide solution. After soaking, wash the steel fiber with water until the washing solution is neutral. Dry the washed steel fiber. Step (A-2): Add the dried steel fibers to the waterborne polyurethane and stir until the surface of the steel fibers is completely submerged in the waterborne polyurethane, to obtain impregnation system A; the waterborne polyurethane is a carboxylic acid polyurethane resin dispersion or a carboxylic acid polyurethane resin emulsion; the mass fraction of carboxylic acid polyurethane resin in the waterborne polyurethane is 50-60 wt%; the mass fraction of carboxyl groups in the carboxylic acid polyurethane resin is 3-5 wt%; the mass ratio of steel fibers to waterborne polyurethane is 1:1-2. Step (A-3): Add zirconium ammonium carbonate solution to impregnation system A under stirring and stir to obtain impregnation system B; the volume ratio of zirconium ammonium carbonate solution added in step (A-3) to waterborne polyurethane in step (A-2) is 1:40-60. Step (A-4): Remove the steel fibers from the impregnation system B, drain them, and place them in a drying oven to dry, thus obtaining pretreated steel fibers; In step B, the amount of pretreated fiber added is 0.10-0.15 wt% of the silica sol mass; the silica content in the silica sol is 20-30 wt%; the pH of the silica sol is 9-10; the ultrasonic frequency is 28 kHz, the ultrasonic power is 600-1000 W, and the ultrasonic stirring time is 0.5-1 h. In step C, the mass ratio of silica sol dispersion to refractory powder is 1:1-1.5; In step (A-1), the sodium hydroxide solution contains 10-20 wt% sodium hydroxide and the soaking time is 30-60 min; the steel fiber length is 2-5 mm and the diameter is 5-10 μm. In step (A-3), the mass fraction of zirconium carbonate in the zirconium carbonate solution is 10-15 wt%. In step (A-4), the drying temperature is 40-60℃ and the drying time is 2-3 hours.

Citation Information

Patent Citations

  • Method for producing leather material and leather material

    CN101994263A

  • Method for preparing fibrilia carboxylation cellulose nanowhiskers

    CN102675475A

  • Preparation method of fiber reinforced compound silica sol shell for investment casting

    CN103962506A