A CsPbBr3 quantum dot Li-Al-Si microcrystalline glass, its preparation method and application

By controlling the growth of CsPbBr3 quantum dots through a microreactor formed in Li-Al-Si glass, the problem of uncontrolled growth in traditional glass matrices is solved, achieving efficient and stable narrowband emission and high quantum efficiency, making it suitable as a green light conversion material for LCD liquid crystal displays.

CN117819826BActive Publication Date: 2026-11-10WENZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311681691.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-08
Publication Date
2026-11-10
Estimated Expiration
2043-12-08

AI Technical Summary

Technical Problem

The growth of CsPbX3 quantum dots in traditional glass matrices is uncontrolled, resulting in broadened emission peaks, low quantum efficiency, and poor stability, which cannot meet the requirements of commercial applications.

Method used

Using Li-Al-Si glass as a carrier, the growth of CsPbBr3 quantum dots was controlled by forming a microreactor in the glass through adjusting the glass composition and heat treatment process, thus preparing CsPbBr3 quantum dot Li-Al-Si microcrystalline glass with high fluorescence quantum yield and narrow band emission.

Benefits of technology

Controllable growth of CsPbBr3 quantum dots was achieved, with an emission peak half-width of less than 20 nm and a fluorescence quantum yield of over 90%. The material exhibits good stability in water and is suitable as a green light conversion material for LCD displays, improving color purity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004596390420000071
    Figure BDA0004596390420000071
  • Figure BDA0004596390420000081
    Figure BDA0004596390420000081
  • Figure HDA0004596390430000011
    Figure HDA0004596390430000011
Patent Text Reader

Abstract

This invention discloses a CsPbBr3 quantum dot Li-Al-Si microcrystalline glass, its preparation method, and its applications. The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass is obtained by melting, water quenching, grinding, and annealing glass powder, which is composed of B2O3, SiO2, Al2O3, K2CO3, Li2CO3, PbBr2, NaBr, and Cs2CO3. The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared by this invention exhibits high fluorescence quantum yield, high stability, and narrow-band emission. This invention provides the application of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass in the preparation of light conversion films for LCD liquid crystal displays. The emission peak half-width at half-maximum (FWHM) of the light conversion film is within 20 nm, greatly improving the color purity of green displays and significantly increasing the color gamut area of ​​LCD displays.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a CsPbBr3 quantum dot glass-ceramic, its preparation method and application, and belongs to the field of quantum dot glass-ceramic. Background Technology

[0002] All-inorganic perovskite CsPbX3 quantum dots have attracted widespread attention and are hailed as a "star" material of our time due to their excellent optical properties, including full-spectrum tunability, narrow emission bands, high quantum yield, and low manufacturing cost. However, CsPbX3 three-dimensional perovskite quantum dots exhibit phase transitions and instabilities, easily deteriorating under the influence of environmental factors such as water, light, and oxygen, thus affecting their optical properties. This has become the biggest bottleneck for their commercial applications. Dense inorganic oxide glass networks have been chosen as carriers to isolate quantum dots from the external environment. The robust and dense glass matrix can effectively suppress the aggregation and color segregation of perovskite quantum dots. Currently, CsPbX3 has been successfully embedded in glass systems such as phosphate, tellurate, borosilicate, borosilicate, and chalcogenide glasses, enabling perovskite quantum dot glasses to begin to show promise in applications such as optical information storage, optical communication, backlight displays, and solid-state lighting. However, in a disordered glass matrix, the control over the growth size, composition, and structure of quantum dots is affected by the original composition of the glass matrix, preventing the perovskite quantum dots embedded in the glass from realizing their full advantages. Quantum dots grown in traditional glass matrices are difficult to control, resulting in a wide size distribution and a broad emission peak. In recent studies, CsPbBr3 quantum dot glasses have achieved quantum efficiencies exceeding 90%, but their emission peaks have a large half-width at half-maximum (FWHM), above 25 nm, leading to lower color purity. Furthermore, in traditional glass matrices, high quantum efficiencies are often achieved at the expense of glass network connectivity. A broken glass network compromises the stability of CsPbBr3 quantum dots; after only 30 days of immersion in water, their luminescence intensity decreases by 10%, failing to meet application requirements. Summary of the Invention

[0003] The purpose of this invention is to provide a CsPbBr3 quantum dot Li-Al-Si microcrystalline glass with high stability, high quantum efficiency, and narrow-band emission, as well as its preparation method and its application in the preparation of green light conversion materials for LCD liquid crystal displays. Li-Al-Si glass, whose composition and structure can be largely adjusted, is selected as the carrier. By adjusting the glass composition and heat treatment process, a microreactor is formed inside the glass to control the growth of CsPbX3, allowing the quantum dots embedded in the glass to maximize their advantages. This achieves high fluorescence quantum yield while further improving stability and reducing the full width at half maximum (FWHM) of the emission peak.

[0004] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0005] In a first aspect, the present invention provides a CsPbBr3 quantum dot Li-Al-Si microcrystalline glass, which is obtained by melting, water quenching, grinding and annealing glass raw materials. The glass raw materials are composed of the following components, wherein the molar fraction of each component is: B2O3 8-35%, SiO2 20-55%, Al2O3 3-10%, K2CO3 0-7%, Li2CO3 15-25%, PbBr2 4-10%, NaBr 3-10% and Cs2CO3 4-7%, and the sum of the molar fractions of each component is 100%.

[0006] The principle of this invention for preparing CsPbBr3 quantum dot Li-Al-Si microcrystalline glass is as follows: In the glass formulation, SiO2 and B2O3 are network forming agents forming the glass matrix, Al2O3 is a network intermediate agent to repair the network, Li2O is a network modifier to fill the network, and PbBr2 and Cs2CO3 are microcrystalline materials. By adjusting the composition of the Li-Al-Si glass and the annealing process, different microreactors are formed in the glass to control the in-situ growth of CsPbBr3 quantum dots in the glass, so as to prepare CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material with high fluorescence quantum yield, high stability, and narrow band emission.

[0007] Preferably, the molar fractions of each component in the glass raw material are: B2O3 10-25%, SiO2 29-50%, Al2O3 4-10%, K2CO3 0-6%, Li2CO3 16-22%, PbBr2 4%, NaBr 4-6%, and Cs2CO3 4-6%. More preferably, the molar fractions of each component in the glass raw material are: B2O3 10-15%, SiO2 43-50%, Al2O3 4-6%, K2CO3 4-6%, Li2CO3 16-18%, PbBr2 4%, NaBr 4%, and Cs2CO3 6%. The most preferred molar fractions of the components in the glass raw material are: B2O3 15%, SiO2 43%, Al2O3 6%, K2CO3 4%, Li2CO3 18%, PbBr2 4%, NaBr 4%, and Cs2CO3 6%.

[0008] The glass raw materials used in this invention have a purity of over 98%.

[0009] Secondly, the present invention provides a method for preparing the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass described in the first aspect, the specific steps of which are as follows:

[0010] (1) B2O3, SiO2, Al2O3, K2CO3, Li2CO3, PbBr2, NaBr and Cs2CO3 were ground and mixed to obtain a mixed powder. The molar fractions of each component in the mixed powder were: B2O3 8-35%, SiO2 20-55%, Al2O3 3-10%, K2CO3 0-7%, Li2CO3 15-25%, PbBr2 4-10%, NaBr 3-10% and Cs2CO3 4-7%, and the sum of the molar fractions of each component was 100%.

[0011] (2) The mixed powder from step (1) is melted at 1200-1400℃ for 1-20 minutes to obtain a melt. The melt is then poured into water and quenched to obtain a precursor glass. The precursor glass is dried and then ground to obtain precursor glass powder.

[0012] (3) The precursor glass powder obtained in step (2) is annealed at a temperature of 400℃-600℃ for 1-20 hours to obtain CsPbBr3 quantum dot Li-Al-Si microcrystalline glass.

[0013] Preferably, in step (2), the temperature is increased to the melting temperature at a rate of 5-10 °C / min.

[0014] Preferably, in step (2), the melting temperature is 1200-1300℃, more preferably 1250℃; and the melting time is 5-15 minutes, more preferably 10 minutes.

[0015] Preferably, in step (2), the drying temperature of the precursor glass is 40-200℃.

[0016] Preferably, in step (2), the grinding of the precursor glass is carried out in a ball mill with a speed of 200-400 rpm and a grinding time of 1-10 hours.

[0017] Preferably, in step (3), the annealing temperature is 450-500℃, more preferably 480℃; and the annealing time is 4-6 hours, more preferably 5 hours.

[0018] The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass prepared by this invention can be used to prepare light conversion materials, and has potential application prospects in fields such as laser projection display, backlight display, optical information storage, optical communication, photodetector, solid-state lighting, X-ray scintillation imaging, microlaser, and solar cell devices.

[0019] Thirdly, the present invention provides the application of the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass described in the first aspect in the preparation of green light conversion materials for LCD liquid crystal displays. The green light conversion material is obtained by mixing the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder with PS masterbatch, followed by co-melting extrusion using a twin-screw extruder, die shaping, and cooling.

[0020] Preferably, the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder and PS masterbatch are mixed at a mass ratio of 1:15.

[0021] Compared with the prior art, the beneficial effects of the present invention are:

[0022] (1) The in-situ crystallization of CsPbBr3 quantum dots in a microreactor formed by Li-Al-Si microcrystalline glass can realize the controllable preparation of CsPbBr3 quantum dots, and to a large extent, the optical properties of CsPbBr3 quantum dots can be tuned. The emission center wavelength can be tuned between 500-530nm, and the emission half width at half maximum can be controlled within 20nm.

[0023] (2) The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared by the present invention has a fluorescence quantum yield of >90%.

[0024] (3) The high-performance CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared by this invention has super water stability. When the prepared microcrystalline glass powder material is soaked in water for 180 days, its fluorescence intensity remains above 90%.

[0025] (3) The preparation method of the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared by the present invention is simple and easy to encapsulate into various light conversion materials.

[0026] (4) The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared in this invention is packaged as a light conversion film and applied to LCD liquid crystal displays. The emission peak half width at half maximum of the light conversion film is within 20nm, which greatly improves the color purity of green display and enables the color gamut area of ​​LCD display to reach 134% of the NTSC 1953 standard and 100% of the Rec.2020 standard.

[0027] (5) The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass material prepared by this invention is suitable for industrialization and has potential application prospects in the fields of laser projection display, backlight display, optical information storage, optical communication, photodetector, solid-state lighting, X-ray scintillation imaging, micro-laser, and solar cell devices. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, obtaining other drawings based on these drawings without creative effort still falls within the scope of the present invention.

[0029] Figure 1 This is a schematic diagram of the preparation process of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass according to the present invention.

[0030] Figure 2 Photographs of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass prepared in Examples 1-6 under white light and 365nm ultraviolet light irradiation.

[0031] Figure 3 Fluorescence spectra of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass prepared in Examples 1-6 under 365nm ultraviolet light excitation, as well as the variation trends of its emission center wavelength and emission peak half-width at half maximum (FWHM).

[0032] Figure 4 XRD patterns of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass prepared in Examples 1-6;

[0033] Figure 5 Absorption spectra of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass prepared in Examples 1-6;

[0034] Figure 6 The trends of fluorescence intensity, fluorescence emission wavelength, and emission peak full width at half maximum (FWHM) of the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder prepared in Example 4 after immersion in water for 180 days;

[0035] Figure 7 The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder prepared in Example 3 was encapsulated as a light conversion film;

[0036] Figure 8 This relates to the color gamut area and display spectrum of the LCD liquid crystal display encapsulated using the aforementioned light conversion film. Detailed Implementation

[0037] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings.

[0038] Examples 1-6

[0039] First, the glass raw materials, with a purity of over 98%, were weighed according to the molar ratios shown in Table 1, mixed thoroughly, and placed in a muffle furnace. The mixture was heated from room temperature to 1250°C over 150 minutes and held for 10 minutes. The molten glass was then water-quenched. After water quenching, the precursor glass was dried at 60°C and then ground in a ball mill at 330 rpm for 4 hours to obtain precursor glass powder. The precursor glass powder was then heat-treated at 480°C for 5 hours to obtain CsPbBr3 quantum dot Li-Al-Si microcrystalline glass.

[0040] Table 1. Mole fractions of raw materials and products for each embodiment.

[0041]

[0042] The prepared CsPbBr3 quantum dot Li-Al-Si microcrystalline glass was ground into powder, and related tests such as photoelectric properties and structural analysis were performed. Figure 2 , Figure 3 , Figure 4 As shown in Table 1. Optimized experimental conditions resulted in XRD peaks corresponding clearly to the standard, confirming the successful preparation of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass. Figure 4 .

[0043] The prepared CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder samples were photographed under white light (top) and 365nm ultraviolet light (bottom), respectively. See the sample images below. Figure 2 .

[0044] The photoluminescence fluorescence spectra of the prepared CsPbBr3 quantum dot Li-Al-Si glass-ceramic samples were measured using a fluorescence spectrometer (Hitachi, F7000) and a xenon lamp (λex = 365 nm). The full width at half maximum (FWHM) and center wavelength of the emission peaks were then obtained using Origin software. The results are shown below. Figure 3 As shown in the figure, as the boron oxide content increases, the emission wavelength of each embodiment gradually red-shifts from 507 nm to 522 nm, and the fluorescence intensity gradually increases, with the fluorescence intensity of Example 4 reaching the highest. The full width at half maximum (FWHM) of the emission peak gradually decreases, with Example 3 reaching the minimum value of 19.5 nm.

[0045] The prepared CsPbBr3 quantum dot Li-Al-Si glass-ceramic powder samples were measured in a Bruker D8 XRD instrument. The Bruker D8 was operated with a Cu-Kα radiation at a 10-60 (2θ) boundary current and a voltage of 40 mA at a velocity of 0.02 s⁻¹. The obtained XRD patterns are shown in Figure 4. As can be seen from the figure, with the increase of boron oxide content, the diffraction peaks of the corresponding CsPbBr3 crystals in each embodiment gradually appeared and became more obvious, proving that the CsPbBr3 crystals were successfully grown in the glass matrix.

[0046] The absorption spectra of the prepared CsPbBr3 quantum dot Li-Al-Si glass-ceramic powder samples were measured using a Varian Cary 5 spectrophotometer (Shimadzu, UV-3600) at room temperature (λex = 365 nm). The results are as follows: Figure 5 As shown in the figure, after the addition of boron oxide, each embodiment exhibits a distinct absorption shoulder peak around 520 nm.

[0047] Table 1 Fluorescence quantum yield

[0048]

[0049] Example 7: Water Stability Test

[0050] The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder sample prepared in Example 4 was immersed in deionized water. After being removed and dried sequentially, its fluorescence spectrum was measured using a fluorescence spectrometer (Hitachi, F7000) and a xenon lamp (λex = 365 nm). The fluorescence intensity, emission peak center wavelength, and full width at half maximum (FWHM) were then processed using Origin software to obtain the corresponding trends. The results are as follows: Figure 6 As shown in the figure, the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder sample prepared in Example 4, after being immersed in water for 180 days, still maintained a fluorescence intensity of over 90%, and its emission peak center wavelength and emission peak half-width at half-maximum showed no significant change.

[0051] Example 8

[0052] The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder obtained in Example 4 was mixed with PS masterbatch at a mass ratio of 1:15. The mixture was then melt-extruded using a twin-screw extruder with a heating range of 190-200°C at 200°C. After molding and cooling, a light conversion film was obtained. Images of this light conversion film under white light (top) and 365nm ultraviolet light (bottom) are shown below. Figure 7 As shown.

[0053] The green light conversion material built into the commercial LCD display was removed, and then replaced with the light conversion film prepared above, encapsulating it into a new LCD display. The color gamut area and emission spectrum of this LCD display were obtained by directly testing the corresponding CIE color coordinates and emission spectrum on the encapsulated display screen using an iridescent colorimeter and then calculating and analyzing the results. Figure 8 As shown in the figure, compared to commercial LCD displays, the LCD display encapsulated with the light conversion film prepared in Example 8 has a narrower half-width at half-maximum (WHM) of the green emission peak, a greener color coordinate, and higher color purity in green display. The color gamut area calculated using CIE color coordinates reaches 134% of the NTSC 1953 standard and 100% of the Rec. 2020 standard, while the commercial display is only 85% of the NTSC 1953 standard.

[0054] The above-disclosed embodiments are merely some examples of the present invention and should not be construed as limiting the scope of the present invention. Therefore, any equivalent variations made in accordance with the claims of the present invention are still within the scope of the present invention.

Claims

1. A CsPbBr3 quantum dot Li-Al-Si microcrystalline glass, obtained from glass raw materials through melting, water quenching, grinding, and annealing, characterized in that: The glass raw material is composed of the following components, wherein the molar fraction of each component is: B2O3 10~25%, SiO2 29~50%, Al2O3 4~10%, K2CO3 0~6%, Li2CO3 16~22%, PbBr2 4%, NaBr 4~6% and Cs2CO3 4~6%.

2. The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass as described in claim 1, characterized in that: The molar fractions of each component in the glass raw material are: B2O3 10~15%, SiO2 43~50%, Al2O3 4~6%, K2CO3 4~6%, Li2CO3 16~18%, PbBr2 4%, NaBr 4%, and Cs2CO3 6%.

3. The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass as described in claim 1, characterized in that: The molar fractions of each component in the glass raw material are: B2O3 15%, SiO2 43%, Al2O3 6%, K2CO3 4%, Li2CO3 18%, PbBr2 4%, NaBr 4%, and Cs2CO3 6%.

4. A method for preparing CsPbBr3 quantum dot Li-Al-Si microcrystalline glass according to any one of claims 1-3, characterized in that: The specific steps of the preparation method are as follows: (1) B2O3, SiO2, Al2O3, K2CO3, Li2CO3, PbBr2, NaBr and Cs2CO3 are ground and mixed to obtain glass powder; (2) Melt the mixed powder from step (1) at 1200-1400℃ for 1-20 minutes to obtain a melt. Pour the melt into water and quench it to obtain a precursor glass. Dry the precursor glass and grind it to obtain precursor glass powder. (3) The precursor glass powder obtained in step (2) is annealed at a temperature of 400℃-600℃ for 1-20 hours to obtain CsPbBr3 quantum dot Li-Al-Si microcrystalline glass.

5. The preparation method according to claim 4, characterized in that: In step (2), the temperature is increased to the melting temperature at a rate of 5-10℃ / min.

6. The preparation method according to claim 4, characterized in that: In step (2), the melting temperature is 1200-1300℃; the melting time is 5-15 minutes.

7. The preparation method according to claim 4, characterized in that: In step (3), the annealing temperature is 450-500℃ and the annealing time is 4-6 hours.

8. The application of CsPbBr3 quantum dot Li-Al-Si microcrystalline glass as described in any one of claims 1-3 in the preparation of green light conversion materials for LCD liquid crystal displays, characterized in that: The green light conversion material is obtained by mixing the CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder with PS masterbatch, followed by co-melting extrusion using a twin-screw extruder, die shaping, and cooling.

9. The application as described in claim 8, characterized in that: The CsPbBr3 quantum dot Li-Al-Si microcrystalline glass powder and PS masterbatch are mixed at a mass ratio of 1:15.

Citation Information

Patent Citations

  • Solid-phase synthesis method of inorganic perovskite quantum dots

    CN109354059A

  • Transparent long-afterglow glass ceramics and preparation method thereof

    CN110156332A