Sliding components and their applications

By adopting a CrAlN/Cr(Al)N multilayer coating structure on the piston rings of internal combustion engines, the problems of insufficient wear resistance and anti-cracking properties in the prior art are solved, achieving higher hardness and wear resistance, and enhancing oxidation resistance at high temperatures.

CN117845166BActive Publication Date: 2026-11-10MAHLE INT GMBH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311259459.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-10-04
Filing Date
2023-09-27
Publication Date
2026-11-10
Estimated Expiration
2043-09-27

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to improve wear resistance, crack resistance and hardness of piston ring coatings for internal combustion engines at the same time, and single-layer nitride coatings cannot meet higher performance requirements.

Method used

A multi-layer protective coating structure is adopted, with alternating layers of CrAlN and Cr(Al)N. The Al content of the CrAlN layer is higher than that of the Cr(Al)N layer. It is formed by physical vapor deposition process. The difference in layer thickness and Al concentration is designed to reduce the interfacial stress gradient and improve the hardness.

Benefits of technology

It significantly improves the wear resistance and anti-cracking properties of sliding components, reduces coating wear, and enhances oxidation resistance and mechanical properties at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117845166B_ABST
    Figure CN117845166B_ABST
Patent Text Reader

Abstract

This invention relates to a sliding member and its use. A sliding member (1) comprises: a metal substrate (2); at least one intermediate bonding layer (3) made of at least one metal and present on the metal substrate (2) in such a way as to cover at least a portion of the surface of the metal substrate (2); and a multilayer protective coating (4) present on the intermediate bonding layer (3), wherein the multilayer protective coating (4) has alternating layers of CrAlN (4a) and Cr(Al)N (4b), wherein every two alternating layers of CrAlN (4a) and Cr(Al)N (4b) form a periodic layer group (4c), the CrAlN layer (4a) has a higher Al content than the Cr(Al)N layer (4b), the thickness ratio of the CrAlN layer (4a) to the Cr(Al)N layer (4b) in each periodic layer group (4c) is 1 < (thickness of CrAlN layer) / (thickness of Cr(Al)N layer) ≤ 10, and the total Al content of the multilayer protective coating (4) is 15 to 40 atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a sliding member, particularly for use in internal combustion engines or compressors, the sliding member having multiple sequential coatings of aluminum-containing chromium nitride. The resulting sliding member achieves excellent wear resistance and spalling resistance. Background Technology

[0002] Internal combustion engines that operate according to the Otto and Diesel cycles are used to traction drive the vast majority of automobiles and basically consist of two main components: the cylinder block (where one or more cylinders and the crankshaft are located) and one or more cylinder heads connected to it. Pistons and connecting rods are connected to the crankshaft.

[0003] The space defined between the piston top surface, cylinder wall and cylinder head bottom corresponds to the combustion chamber. In diesel engines, the combustion chamber is usually defined by one or more cavities located on the piston head.

[0004] Inside the combustion chamber, the engine converts the chemical energy from the combustion of the combustible mixture (fuel and air) into mechanical energy that can transfer motion to the wheels.

[0005] To ensure even combustion and prevent oil burning, and also to avoid excessive gas from the cylinder to the crankcase, it is necessary to use rings to provide a good seal between the piston and the cylinder wall.

[0006] Typically, modern four-stroke engines use three rings on each piston: two compression rings and one oil ring. The compression rings prevent combustion gases from reaching the crankcase, while the oil rings scrape excess oil from the cylinder walls and return it to the crankcase, control the thickness of the oil "film," and prevent it from being overburned.

[0007] Another important function of the ring is to act as a bridge to transfer heat from the piston to the cylinder wall / sleeve, where the heat is dissipated by the cooling system.

[0008] As a general principle, piston rings, especially compression rings, are formed from a metal substrate coated with at least one coating that is in contact with the cylinder wall.

[0009] The coating plays a crucial role because it aims to impart low sliding wear properties, excellent anti-split fracture properties, hardness, and toughness to the ring. However, many of these properties are contradictory, and an increase in one often results in a compromise in the performance of another. Therefore, the type of coating to be used is selected based on the function of the engine's working profile and the forces the ring experiences during its service life.

[0010] Those skilled in the art have proposed a series of complex coatings, each seeking to enhance desired properties. However, coatings proposed to date have not been effective in simultaneously improving internal stress absorption, achieving excellent hardness and low thickness, thereby significantly reducing spalling.

[0011] The first prior art is represented by U.S. Patent No. 5,718,437, which relates to an oil scraper ring having a Cr2N monolayer coating with a thickness of about 3 μm to 30 μm.

[0012] According to the literature, the Cr2N coating provides a hardness between 1300 HV and 2000 HV and is applied by a process commonly referred to by those skilled in the art as "ion plating".

[0013] The second prior art is represented by Japanese Patent JP 9196173, whose disclosed invention is very similar to US Patent No. 5,718,437, namely an oil scraper ring having a Cr2N single-layer coating with a width of about 3μm to 30μm.

[0014] Furthermore, U.S. Patent No. 5,820,131 relates to a piston ring having a coating with a width of 3 μm to 30 μm formed from a single layer of Cr2N or a single layer of a mixture of Cr2N and CrN, and the nitrogen content by weight is between 11% and 17%. The coating is applied by a process known as physical vapor deposition (PVD), and its hardness ranges from 1300 HV to 2000 HV.

[0015] U.S. Patent No. 5,743,536 relates to a piston ring having a coating at least formed of chromium nitride, said coating being applied by PVD. The chromium nitride comprises CrN, Cr2N, or a mixture of CrN and Cr2N in a single phase. The document also specifies various values ​​for thickness and porosity, and discloses various mechanical tests on products with coatings having various end arrangements. According to this patent, the coating exhibits excellent resistance to wear, spalling, and burning.

[0016] In addition, WO 2005 / 121403 A1 discloses a piston ring comprising a multilayer PVD coating containing multiple Cr / CrN (Cr2N) layers.

[0017] Finally, U.S. Patent No. 6,631,907 relates to a piston ring having a coating applied by PVD comprising a mixture of CrN or Cr2N, or nitrides. This document also discloses the application of mixtures of CrN with Cr2N and metallic chromium, and provides details of the weight percentages of these components.

[0018] Therefore, all the solutions in the prior art mentioned above involve using CrN or Cr2N itself or a mixture thereof to obtain a single-layer coating with a high level of wear resistance, spalling resistance and flammability.

[0019] However, existing proposals have limitations regarding further improvements in wear resistance, spalling resistance, and flammability, which vary depending on the percentage of CrN or Cr2N in the nitride layer and any other elements added. A single-layer nitride coating is not a viable solution if greater improvements in these properties are desired. Summary of the Invention

[0020] Therefore, the object of the present invention is to provide a sliding member having a chromium nitride-based coating that provides further improved wear resistance and spalling resistance.

[0021] The objective is achieved through the subject of independent item 1. An advantageous implementation is through the subject of dependent items.

[0022] The present invention is based on the general idea of ​​using a multilayer protective coating on a metal substrate, wherein the multilayer protective coating has alternating layers of CrAlN and Cr(Al)N, wherein each CrAlN layer has a higher Al content than each Cr(Al)N layer, and the thickness of each CrAlN layer is greater than the thickness of each Cr(Al)N layer.

[0023] CrAlN is known for its passivation properties due to the interstitial Al elements and its high hardness. Sliding components of internal combustion engines, such as piston rings, require coatings with low friction, wear resistance, and high resistance to spalling and abrasion. Higher coating hardness is expected to achieve even greater wear resistance.

[0024] The inventors have discovered a novel CrAlN / Cr(Al)N multilayer film concept, wherein the alternating layers, as described above, have different Al concentrations, resulting in significantly improved wear resistance of the multilayer. Furthermore, due to this multilayer concept, high spalling resistance is achieved because each layer acts as a barrier to dislocation movement. Moreover, high scratch resistance is achieved by the thinner Cr(Al)N layers with low Al content.

[0025] Another advantage of the multilayer concept of this invention is the reduction of the volume of interdiffusion of elements at the layer interfaces, because, in the manner described above, layers with different Al concentrations also have different thicknesses. This specific structure influences the energy adsorption and relaxation dynamics in the elastic regime, plastic deformation, crack initiation, and propagation.

[0026] Furthermore, the multilayer concept is based on the continuous adaptation of lattice parameters, which in turn is based on the continuous adaptation of the energy states (sizes) of the lattice. Therefore, for example, the stress gradient calculated at the coherent interface of CrAlN / Cr(Al)N is lower than that of pure CrN / CrAlN. In this multilayer concept, the coherent strengthening hinders dislocation movement based on the interaction between the interface coherent stress and the elastic stress field of dislocations. The multilayer concept takes into account the compositional gradient and lattice parameter variations within the layers. Elimination of the core region eliminates free crack propagation because there is no stress gradient in the core region.

[0027] Furthermore, the multilayer concept reduces the difference in lattice parameters and thus the maximum residual stress value by maintaining the same periodic thickness for pairs of layers with different Al concentrations, thereby reducing the overall hardness of the coating and mitigating any high wear on the friction-corresponding portions. Additionally, reducing the thickness of one of the layers (the Cr(Al)N layer) will increase the average stress gradient, which manifests as intrinsic elastic stress, believed to be caused by compositional differences and corresponding variations in lattice parameters.

[0028] Both stress amplitude and stress gradient can affect hardness. Therefore, a steeper stress gradient may make dislocation movement more difficult. The smaller the periodic thickness, the greater the stress gradient generated near the interface, and the larger the stress barrier that hinders dislocation movement.

[0029] The incorporation of Al into CrN promotes higher hardness, thermal stability, and chemical stability. This multilayer concept can also increase the hardness and toughness of the coating.

[0030] Finally, the low concentration of Al in the overall coating enables the formation of a metastable Al solution within the face-centered cubic (fcc) CrN lattice, which increases hardness. The CrAlN phase forms a dense and adherent mixed Al and Cr oxide skin, which ultimately inhibits oxygen diffusion into the coating, providing excellent oxidation resistance up to temperatures up to 900°C. Furthermore, the addition of Al as a reactive element is believed to reduce the accumulation of voids at the bulk / skin interface (oxide film), thereby improving the mechanical properties of the coating or preventing grain coarsening at elevated temperatures by altering its structure.

[0031] In view of the above effects, the new multilayer concept of the present invention provides a sliding member that has significantly improved wear resistance and anti-cracking properties compared with the prior art concept.

[0032] In particular, the present invention provides a sliding member comprising: a metal substrate; at least one intermediate bonding layer made of at least one metal and present on the metal substrate in such a manner as to cover at least a portion of the surface of the metal substrate; and a multilayer protective coating present on the intermediate bonding layer, wherein the multilayer protective coating has alternating layers of CrAlN and Cr(Al)N, wherein every two alternating layers of CrAlN and Cr(Al)N form a periodic layer group, the CrAlN layer having a higher Al content than the Cr(Al)N layer, the thickness ratio of the CrAlN layer to the Cr(Al)N layer in each periodic layer group being 1 < (thickness of CrAlN layer) / (thickness of Cr(Al)N layer) ≤ 10, and the total Al content of the multilayer protective coating being 15 to 40 atoms.

[0033] According to a preferred embodiment of the invention, the metal substrate is made of steel having 10 to 17% Cr by weight, carbon steel, or cast iron having a composition typically used in sliding components of internal combustion engines or compressors. However, the invention is not limited to the material used for the metal substrate, and other materials may be used.

[0034] According to a preferred embodiment of the invention, the metal substrate is nitrided. The nitriding can be performed by known methods such as gas nitriding, salt bath nitriding, or plasma nitriding, and results in surface hardening of the metal substrate, improving its overall wear resistance.

[0035] According to a preferred embodiment of the invention, the at least one intermediate bonding layer is made of at least one selected from the group consisting of Cr, Ni, and Co, preferably Cr. The intermediate bonding layer improves the adhesion of the multilayer protective coating. The intermediate bonding layer and the functional coating applied to the metal substrate material are produced, for example, by a physical vapor deposition (PVD) process.

[0036] According to a preferred embodiment of the present invention, the total thickness of the at least one intermediate bonding layer and the multilayer protective coating is 6. m to 70 m, preferred 6 m to 60 m, more preferably 10 m to 50 m. The layer thickness of this sliding member is measured, for example, by cross-sectional evaluation.

[0037] According to a preferred embodiment of the invention, in each periodic layer group, the thickness ratio of the CrAlN layer to the Cr(Al)N layer is 1.3 to 10, preferably 1.5 to 10, more preferably 1.7 to 10, even more preferably 1.5 to 5, and particularly 1.7 to 5.

[0038] According to a preferred embodiment of the invention, the CrAlN layer contains 20 to 40 atomic% Al, preferably 25 to 35 atomic% Al, more preferably 27 to 32 atomic% Al, and the Cr(Al)N layer contains 10 to 25 atomic% Al, preferably 15 to 22 atomic% Al, more preferably 18 to 20 atomic% Al. For example, the chemical composition can be measured by EELS (electron energy loss spectroscopy) or EDS (energy dispersive spectroscopy).

[0039] According to a preferred embodiment of the invention, the thickness of each periodic layer group is less than 20 nm, preferably less than 18 nm, more preferably less than 15 nm, and particularly 5 to 15 nm.

[0040] According to a preferred embodiment of the present invention, the hardness of the multilayer protective coating is 1600 to 2600 HV, preferably 1800 to 2400 HV, and more preferably 1900 to 2000 HV.

[0041] According to a preferred embodiment of the present invention, the internal compressive stress of the multilayer protective coating is measured by X-ray analysis to be 1000 to 2500 MPa, preferably 1200 to 2300 MPa, and more preferably 1400 to 2000 MPa.

[0042] According to a preferred embodiment of the present invention, the cross-sectional image of the coating is measured by analysis software, and the porosity of the multilayer protective coating is less than 6%, preferably less than 5%, more preferably less than 4%, and particularly less than 3%.

[0043] According to a preferred embodiment of the present invention, the multilayer protective coating is formed by cathodic arc deposition. Methods and apparatus for cathodic arc deposition are well known to those skilled in the art. Specific cathodic arc deposition methods and corresponding apparatus are further discussed below.

[0044] Furthermore, the present invention provides the use of sliding members in internal combustion engines or compressors, wherein the sliding member is preferably a piston ring, tappet, valve, or cam. Other specific examples of the claimed uses of the sliding member are oil scraper rings, compression rings in two-stroke engines, and rings in piston compressors.

[0045] Other important features and advantages of the invention are derived from the dependent items, the accompanying drawings, and the corresponding descriptions of the drawings.

[0046] It should be noted that the features described above and discussed below can be used not only in the corresponding given combinations, but also in different combinations or such combinations that do not exceed the scope of the invention. Attached Figure Description

[0047] Preferred embodiments of the present invention are shown in the accompanying drawings and are further discussed in the following description, wherein like reference numerals refer to similar or functionally identical components.

[0048] The diagram schematically illustrates: Figure 1 A cross-sectional view of the sliding member (1) of the present invention includes a metal substrate (2), an intermediate bonding layer (3), and multiple CrAlN and Cr(Al)N layers (4a, 4b) forming a multilayer protective coating (4). Figure 2 A schematic top view of a cathode arc deposition apparatus suitable for manufacturing the multilayer protective coating (4) of the present invention. Figure 3 The sliding member (1) of the present invention in the form of a piston ring, and Figure 4 A bar graph used to compare the relative wear of prior art protective coatings and multilayer protective coatings according to the present invention. Detailed Implementation

[0049] according to Figure 1 A cross-sectional view of the sliding member (1) of the present invention includes a metal substrate (2), an intermediate bonding layer (3) present on the metal substrate (2), and a plurality of CrAlN and Cr(Al)N layers (4a, 4b) on the intermediate bonding layer (3) forming a multilayer protective coating (4). The plurality of CrAlN and Cr(Al)N layers (4a, 4b) are alternately arranged on the intermediate bonding layer (3), wherein the layer immediately above the intermediate bonding layer (3) is a CrAlN layer (4a). However, starting with a CrAlN layer (4a) is not mandatory, that is, the first layer on the intermediate bonding layer (3) may also be a Cr(Al)N layer (4b). According to the present invention and as follows Figure 1 As schematically shown above, the thickness of the CrAlN layer (4a) is set to be greater than the thickness of the Cr(Al)N layer (4b). Furthermore, according to the present invention, as described above, the Al concentration in the CrAlN layer (4a) is set to be greater than the Al concentration in the Cr(Al)N layer (4b). Every two alternating CrAlN and Cr(Al)N layers (4a, 4b) form a periodic layer group (4c), as shown in the diagram. Figure 1 The two bottommost CrAlN and Cr(Al)N layers (4a, 4b) are exemplarily indicated.

[0050] Figure 2 A schematic top view of a cathode arc deposition apparatus suitable for manufacturing the multilayer protective coating (4) of the present invention is shown.

[0051] Nitride multilayers, such as CrAlN / Cr(Al)N used in this invention, are isomorphous and miscible. The mixing of these components is confined to occur during deposition by the PVD (physical vapor deposition) chamber configuration, resulting in a compositional gradient. The degree of mixing varies with deposition conditions, particularly regarding cross-contamination between targets during the process, and is primarily due to the individual target compositions (e.g., in this case, one half of the target has a high Al content in the range of 50 to 75 atomic percent, while the other half has Al in the range of 3 to 10 atomic percent).

[0052] according to Figure 2 As an example of manufacturing the sliding component of the present invention, a multilayer protective coating of CrAlN / Cr(Al)N nanostructures was deposited on a gas-nitrided martensitic stainless steel (AISI 440B) specimen (5) by cathodic arc physical vapor deposition (CAPVD) in an industrial-sized chamber (6). Two cathodes in alternating positions [one set of Cr(Al)(7b) with an Al content of 3 to 10 atomic% and one set of CrAl(7a) with an Al content of 50 to 75 atomic%] were powered by their own power sources. By varying the rotational speed of the stage (8) located in the center of the chamber (6), a coating thickness of 30 µm was obtained, with a periodic layer group (4c) thickness of less than 15 nm. The rotational speed controlled the time the substrate passed in front of each CrAl or Cr(Al) target (7a, 7b) in a manner that controlled the periodic thickness, ensuring a significant reduction in cross-contamination between the targets. The average deposition rate for all deposits was 5. m / h.

[0053] Figure 3 The sliding member (1) of the present invention is shown in the form of a piston ring, which can be manufactured by CAPVD as discussed above. Figure 3 The piston ring comprises a metal substrate (2) (only a ring segment of the piston ring is shown), an intermediate bonding layer (3) on the outer ring surface of the metal substrate (2), and a multilayer protective coating (4) on the intermediate bonding layer (3).

[0054] at last, Figure 4Bar graphs are shown comparing the relative wear of prior art protective coatings and multilayer protective coatings according to the present invention. All engine tests were conducted on an HDD platform with a bore diameter of 128 mm, power ranging from 320 to 370 kW, and durations from 250 to 1,000 hours. The first bar shows the results of a prior art multilayer coating structure consisting of NbN / CrN with a periodicity of 20 nm (in a 1:1 ratio of 10 nm NbN and 10 nm CrN), while the second bar shows a CrAlN monolayer coating (without multilayers), and the final third bar shows the results of a multilayer CrAlN / Cr(Al)N coating with a periodicity of 20 nm and a 1:1 ratio.

[0055] like Figure 4 The remaining four bars, surrounded by rectangles, show the tests conducted on the CrAlN / Cr(Al)N variant according to the invention. The results showed a significant reduction in total wear of the coating.

Claims

1. A sliding member, the sliding member comprising: Metal substrate; At least one intermediate bonding layer, the intermediate bonding layer being made of at least one metal and existing on the metal substrate in such a way as to cover at least a portion of the surface of the metal substrate; and A multilayer protective coating exists on the intermediate bonding layer, wherein The multilayer protective coating has alternating first and second layers, both of which are composed of aluminum-containing chromium nitride, and each pair of alternating first and second layers forms a periodic layer group. The first layer has a higher Al content than the second layer. In each periodic layer group, the thickness ratio of the first layer to the second layer is >1 and ≤10. The total Al content of the multilayer protective coating is 15% to 40 atomic%. The total thickness of the at least one intermediate bonding layer and the multilayer protective coating is 6 μm to 70 μm. The hardness of the multilayer protective coating is 1600 to 2600 HV, and The porosity of the multilayer protective coating is less than 6%.

2. The sliding member according to claim 1, wherein the metal substrate is made of steel, carbon steel or cast iron having 10 to 17% Cr by mass.

3. The sliding member according to claim 2, wherein the metal substrate is nitrided.

4. The sliding member according to any one of claims 1 to 3, wherein the at least one intermediate bonding layer is made of at least one selected from the group consisting of Cr, Ni and Co.

5. The sliding member according to any one of claims 1 to 3, wherein in each periodic layer group, the thickness ratio of the first layer to the second layer is 1.3 to 10.

6. The sliding member according to any one of claims 1 to 3, wherein the first layer contains 20 to 40 atomic% Al and the second layer contains 10 to 25 atomic% Al.

7. The sliding member according to any one of claims 1 to 3, wherein the thickness of each periodic layer group is less than 20 nm.

8. The sliding member according to claim 7, wherein the thickness of each periodic layer group is 4 to 15 nm.

9. The sliding member according to any one of claims 1 to 3, wherein the internal compressive stress of the multilayer protective coating is 1000 to 2500 MPa.

10. The sliding member according to any one of claims 1 to 3, wherein the multilayer protective coating is formed by cathodic arc deposition.

11. Use of the sliding member according to any one of claims 1 to 10 in an internal combustion engine or compressor.

12. The use according to claim 11, wherein the sliding member is a piston ring, tappet, valve, or cam.

Citation Information

Patent Citations

  • Combined oil ring with spacer / expander having Cr2N coating thereon

    US5718437A

  • Piston ring

    US5743536A

  • Piston ring having wear coating consisting of Cr2N or a mixture of Cr2N and Cr

    US5820131A

  • Nitride-plated piston ring for internal combustion engines

    US6631907B1

  • Structural gliding component

    WO2005121403A1