A fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers

By using fiber-modified reinforced phase laser cladding composite powder, the problem of uneven mechanical properties caused by ceramic particle deposition was solved, achieving uniformity and improved wear resistance of metal-based composite coatings, and reducing manufacturing costs.

CN117845208BActive Publication Date: 2026-11-17XIAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410059074.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2026-11-17
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

In existing technologies for preparing ceramic particle-reinforced metal matrix composite coatings, ceramic particles are prone to deposition, leading to uneven mechanical properties and affecting the coating's performance.

Method used

A fiber-modified reinforced phase laser cladding composite powder, including cobalt-based alloy powder, carbon nanotube powder, and carbide ceramic powder, was prepared by vacuum drying, ball milling, and sieving to produce a uniformly distributed composite powder. The powder was then laser clad onto the surface of low-carbon steel, with argon gas used as the powder feeder and protective gas.

Benefits of technology

This method achieves uniformity of mechanical properties in metal-based composite coatings, improves production efficiency, reduces manufacturing costs, and enhances the wear resistance and hardness of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117845208B_ABST
    Figure CN117845208B_ABST
Patent Text Reader

Abstract

This invention discloses a fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers. The preparation method includes: Step 1, weighing 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 10-25% carbide ceramic powder, with the sum of the mass percentages of the above components being 100%; Step 2, uniformly mixing the composite powder obtained in Step 1 and drying it in a vacuum tube furnace, maintaining the temperature after drying, and then cooling it to room temperature; Step 3, mixing the composite powder dried in Step 2 and then performing particle size sieving to obtain the fiber-modified reinforced phase laser cladding composite powder; placing the fiber-modified reinforced phase laser cladding composite powder into the powder feeding device of a laser cladding machine, performing laser cladding on low-carbon steel, and cooling to obtain the desired wear-resistant cladding layer; the cladding layer has good forming quality, excellent friction resistance, uniform mechanical properties, fine microstructure, and significantly improved hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of laser cladding technology, specifically relating to a fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers. Background Technology

[0002] With the application and promotion of surface modification technology in traditional steel materials, coatings using various high-performance metals as protective substrates have been extensively studied. However, due to the limited performance and high cost of high-performance metal coatings, metal-based composite coatings have emerged. These are made by adding extremely hard ceramic particles to alloys, possessing good metallurgical compatibility between metals and high wear resistance. Ceramic particle-reinforced metal-based composite coatings can improve the overall performance of the substrate and extend its service life, and have been widely used in various harsh working conditions, such as turbine blades, power generation facilities, and the chemical industry. Laser cladding technology, with its high power, small heat-affected zone, stable light source energy, good surface forming quality, and high degree of automation, has become the best solution for composite coating preparation.

[0003] Currently, commonly used reinforcing phases for preparing ceramic particle-reinforced MMC coatings include metal oxide ceramic phases, metal carbide ceramic phases, and rare earth oxide ceramic phases. The added ceramic reinforcing phases recombine and reorganize within the coating under the convection effect during the cladding process. The nanophase can provide heterogeneous nucleation sites for the growth of other compounds during cladding, interrupting the epitaxial growth of crystals, promoting grain refinement, and improving coating performance. Furthermore, it affects the fluidity of the molten pool, reduces stress concentration in the coating, lowers the coating defect rate, and improves the uniformity of the coating structure. However, due to the significant differences in physical properties such as density between ceramic particles and the cladding metal, and the tendency of ceramic particles to agglomerate (easily settling at the bottom or concentrating at the top), the non-uniformity of mechanical properties in the preparation of metal-based composite coatings actually deteriorates the performance of the cladding layer. Therefore, how to efficiently prepare metal-based composite cladding layers with uniform mechanical properties is a pressing problem to be solved in the field of surface engineering technology. Summary of the Invention

[0004] This invention provides a fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers, its preparation method, and its application. While ensuring the performance of the metal-based composite coating, it homogenizes the mechanical properties of the cladding layer, accelerates production efficiency, and reduces manufacturing costs.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A fiber-modified reinforcing phase laser cladding composite powder for wear-resistant cladding layers comprises 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 10-25% carbide ceramic powder, wherein the sum of the mass percentages of the above components is 100%.

[0007] Furthermore, the cobalt-based alloy powder is Stellite6 with a sphericity of 95%–100%; the carbon nanotube powder has a purity >99%, an inner diameter of 3–5 nm, an outer diameter of 8–15 nm, and a length of 8–14 nm; and the carbide ceramic powder is either B4C or TiC.

[0008] A method for preparing fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers specifically includes the following steps:

[0009] Step 1: Weigh out 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 10-25% carbide ceramic powder by mass percentage, with the sum of the mass percentages of the above components being 100%.

[0010] Step 2: Mix the composite powder prepared in Step 1 evenly and place it in a vacuum tube furnace to dry. After drying, keep it at a warm temperature and then cool it to room temperature.

[0011] Step 3: Mix the composite powder dried in Step 2, and then perform particle size sieving to obtain fiber-modified reinforced phase laser cladding composite powder.

[0012] Further, the specific procedure for step 2 is as follows: the composite powder mixed in step 1 is placed in a tube furnace for drying, 99.9% Ar gas is introduced into the tube furnace, the drying temperature is 110℃~120℃, and the drying time is 30min~60min.

[0013] Furthermore, the specific method for mixing in step 3 is as follows: the composite powder obtained in step 2 is poured into a planetary ball mill without adding grinding balls, the speed is 200-300 rpm, the mill is milled for 1 hour, the interval between shutdowns is 15 minutes, and then the mill is milled for another hour, with the protective gas being 99.9% Ar gas.

[0014] Furthermore, the specific procedure for particle size sieving in step 3 is as follows: the mixed composite powder is poured onto the assembled screen, vibrating screen and screen bottom, the vibrating screen is started for sieving, the sieving time is 5-10 minutes, and composite powder with a size of 15-50μm is screened out.

[0015] The application of fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layer in laser cladding involves placing the fiber-modified reinforced phase laser cladding composite powder into the powder feeding device of a laser cladding machine, performing laser cladding on low carbon steel and cooling it to obtain the desired wear-resistant cladding layer.

[0016] Furthermore, the laser cladding process parameters are as follows: scanning speed of 4mm / s to 5mm / s, laser power of 850W to 1050W, spot diameter of 4mm, and both the protective gas and the powder feeding gas are 99.9% Ar gas.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) The laser cladding method used in this invention is used to clad the surface of low carbon steel. There is less welding spatter during the laser cladding process. Argon gas is used as the powder feeding gas and protective gas to effectively transport the cladding composite powder and protect the cladding layer from gas oxidation. The cladding forming quality is high and the production efficiency is high.

[0019] (2) The fiber-modified reinforced phase laser cladding powder of the present invention has a simple production process, is easy to operate, has high controllability of composition, is flexible in adjustment, has low cost, and can achieve continuous production.

[0020] (3) Multi-walled carbon nanotubes are an allotrope of crystalline carbon. Due to their tendency to aggregate into bundles or entangle, their surface is relatively "inert" compared to other nanoparticles. The encapsulation of carbon nanotubes can effectively reduce the van der Waals forces between ceramic reinforcing phases, eliminate agglomeration, and make the reinforcing phase powder uniformly dispersed. This results in uniform mechanical properties of the metal-based composite cladding layer. Furthermore, the uniform distribution of the reinforcing phase can provide more heterogeneous nucleation and refine the grains.

[0021] (4) Ceramic particles have high hardness, wear resistance and corrosion resistance. Their addition can effectively improve the overall hardness of the cladding layer. The decomposition of some ceramic particles can provide strengthening elements for the cladding layer. Incompletely dissolved fine ceramic particles can act as heterogeneous nucleation points to interrupt dendrite growth and effectively refine the grain size of the cladding layer. Attached Figure Description

[0022] Figure 1 This is a graph showing the wear amount of the wear-resistant cladding layer of this invention;

[0023] Figure 2 This is a hardness cloud diagram of the wear-resistant cladding layer in Embodiment 1 of the present invention;

[0024] Figure 3 This is a hardness cloud diagram of the wear-resistant cladding layer in Embodiment 2 of the present invention;

[0025] Figure 4 This is the hardness cloud diagram of the wear-resistant cladding layer in Embodiment 3 of the present invention;

[0026] Figure 5 This is a metallographic diagram of the interface between the wear-resistant cladding layer and the substrate in Embodiment 1 of the present invention;

[0027] Figure 6 This is a metallographic diagram of the interface between the wear-resistant cladding layer and the substrate in Embodiment 2 of the present invention;

[0028] Figure 7 This is a metallographic diagram of the interface between the wear-resistant cladding layer and the substrate in Embodiment 3 of the present invention. Detailed Implementation

[0029] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.

[0030] A fiber-modified reinforcing phase laser cladding composite powder for wear-resistant cladding layers comprises 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 15% carbide ceramic powder, with the sum of the mass percentages of the above components being 100%. The cobalt-based alloy powder is Stellite6 with a sphericity of 95%-100%; the carbon nanotube powder has a purity >99%, an inner diameter of 3-5 nm, an outer diameter of 8-15 nm, and a length of 8-14 nm; and the carbide ceramic powder is either B4C or TiC.

[0031] A method for preparing fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers specifically includes the following steps:

[0032] Step 1: Weigh out 60-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 15% carbide ceramic powder by mass percentage, with the sum of the mass percentages of the above components being 100%.

[0033] Step 2: Mix the composite powder prepared in Step 1 evenly and place it in a vacuum tube furnace for drying. 99.9% Ar gas is introduced into the tube furnace. The drying temperature is 110℃~120℃ and the drying time is 30min~60min. After drying, keep it at the heat and cool it to room temperature.

[0034] Step 3: Mix the composite powder dried in Step 2, and then perform particle size sieving to obtain fiber-modified reinforced phase laser cladding composite powder.

[0035] The specific method of mixing is as follows: pour the composite powder obtained in step 2 into a planetary ball mill without adding grinding balls, rotate at 200-300 rpm, ball mill for 1 hour, stop for 15 minutes, and then ball mill for another hour. The protective gas is 99.9% Ar gas.

[0036] The specific procedure for particle size sieving is as follows: Pour the mixed composite powder into the assembled screen, vibrating screen and screen bottom, start the vibrating screen for sieving, and the sieving time is 5-10 minutes to screen out composite powder with a particle size of 15-50μm.

[0037] An application of fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers in laser cladding is described. The fiber-modified reinforced phase laser cladding composite powder is placed in the powder feeding device of a laser cladding machine, laser cladding is performed on low-carbon steel, and then cooled to obtain the desired cladding layer. The laser cladding process parameters are: scanning speed of 4mm / s to 5mm / s, laser power of 850W to 1050W, spot diameter of 4mm, and both the protective gas and the powder feeding gas are 99.9% Ar gas.

[0038] Example 1

[0039] Step 1: Weigh the composite powder according to the following mass percentages: 670% Stellite (95%–100% sphericity); 8% carbon nanotube powder (purity >99%, inner diameter 3–5 nm, outer diameter 8–15 nm, length 8–14 nm); and 22% TiC powder. The sum of the mass percentages of the above components is 100%.

[0040] Step 2: After the composite powder is prepared and mixed evenly, it is placed in a vacuum tube furnace for heating and drying, and then cooled to room temperature to obtain the composite powder. 99.9% Ar gas is introduced into the vacuum tube furnace, the drying temperature is 110℃, and the drying time is 30 minutes.

[0041] Step 3: Pour the dried composite powder into a planetary ball mill without adding grinding balls, and ball mill at 200 rpm for 1 hour. Stop the mill for 15 minutes, then ball mill for another hour. The protective gas is 99.9% Ar gas. Then pour the mixed powder onto the assembled sieve, vibrating screen, and sieve bottom. Start the vibrating screen for sieving for 5 minutes, selecting fiber-modified reinforcing phase laser cladding composite powder with a diameter of 15–50 μm.

[0042] The fiber-modified reinforced phase laser cladding composite powder was placed in the powder feeding device of the laser cladding machine, and arc cladding was performed on 45 steel and then cooled. The laser cladding process parameters were: scanning speed of 4 mm / s, laser power of 850 W, spot diameter of 4 mm, and both the protective gas and the powder feeding gas were 99.9% Ar gas, resulting in a wear-resistant cladding layer.

[0043] The wear-resistant cladding layer was subjected to room temperature dry tribology tests under non-vacuum conditions. The friction mode was linear reciprocating motion, the load was 15 N, the friction pair material was Si3N4 ceramic balls, and the friction time was 30 min. Figure 1 The wear amount of the unmodified Q235 steel is 65.3 mg, while that of the wear-resistant cladding layer is 2.3 mg. Wear amount directly reflects the degree of friction of the material; lower wear amount indicates better abrasion resistance. The cobalt-based wear-resistant layer shows a significant improvement in abrasion resistance compared to the substrate. The microhardness of the wear-resistant cladding layer was measured under a load of 1000 N for 15 seconds at a measurement interval of 0.10 mm. The measurement results are shown below. Figure 2 The wear-resistant cladding layer shown exhibits relatively small differences in hardness distribution across different parts, and its hardness is significantly higher than that of the substrate. The microstructure of the wear-resistant cladding layer is as follows: Figure 5The material is mainly composed of columnar crystals with a fine, uniform, and dense structure. There are no obvious defects such as pores or cracks at the interface, which shows that the wear-resistant cladding layer and the substrate have good bonding. Combined with friction and wear test, microhardness test and metallographic analysis at the interface, the wear-resistant cladding layer of the present invention has excellent friction resistance. The reinforcing phase of the prepared cladding layer is uniformly distributed and there is no large regional difference in mechanical properties.

[0044] Example 2

[0045] Step 1: Weigh the composite powder according to the following mass percentages: 75% Stellite6 powder with sphericity of 95%–100%; 8% carbon nanotube powder with purity >99%, inner diameter 3–5 nm, outer diameter 8–15 nm, and length 8–14 nm; and 18% B4C ceramic powder. The sum of the mass percentages of the above components is 100%.

[0046] Step 2: After the composite powder has been prepared, mix it evenly and place it in a vacuum tube furnace for heating and drying, then cool it to room temperature. 99.9% Ar gas is introduced into the vacuum tube furnace, the drying temperature is 110℃, and the drying time is 45 minutes.

[0047] Step 3: Pour the dried composite powder into a planetary ball mill without adding grinding balls, and ball mill at 250 rpm for 1 hour. Stop the mill for 15 minutes, then ball mill for another hour. The protective gas is 99.9% Ar gas. Then pour the mixed powder onto the assembled sieve, vibrating screen, and sieve bottom. Start the vibrating screen for sieving for 10 minutes, selecting fiber-modified reinforced phase laser cladding composite powder with a diameter of 15–50 μm.

[0048] The fiber-modified reinforced phase laser cladding composite powder was placed in the powder feeding device of the laser cladding machine, and arc cladding was performed on 45 steel and then cooled. The laser cladding process parameters were: scanning speed of 5 mm / s, laser power of 950 W, spot diameter of 4 mm, and both the protective gas and the powder feeding gas were 99.9% Ar gas. The target corrosion-resistant and friction-resistant wind turbine blade bearing surface modification structure was obtained.

[0049] The wear-resistant cladding layer was subjected to room temperature dry tribology tests under non-vacuum conditions. The friction mode was linear reciprocating motion, the load was 15 N, the friction pair material was Si3N4 ceramic balls, and the friction time was 30 min. Figure 1 The wear resistance of the unmodified Q235 steel is 65.3 mg, while that of the wear-resistant cladding is 4.3 mg. Wear resistance directly reflects the degree of friction of the material; lower wear resistance indicates better abrasion resistance. The wear-resistant cladding shows a significant improvement in abrasion resistance compared to the substrate. The microhardness of the wear-resistant cladding was measured under a load of 1000 N for 15 seconds at a measurement interval of 0.10 mm. The measurement results are shown below. Figure 3The wear-resistant cladding layer shown exhibits relatively small differences in hardness distribution across different parts, and its hardness is significantly higher than that of the substrate. The microstructure of the wear-resistant cladding layer is as follows: Figure 6 The structure shown is mainly composed of columnar crystals, with a fine, uniform, and dense structure. There are no obvious defects such as pores or cracks at the interface, which shows that the wear-resistant cladding layer and the matrix are well bonded. Combined with friction and wear test, microhardness test and metallographic analysis at the interface, the wear-resistant cladding layer of the present invention has excellent friction resistance. The reinforcing phase of the prepared wear-resistant cladding layer is uniformly distributed and there is no large regional difference in mechanical properties.

[0050] Example 3

[0051] Step 1: Weigh the composite powder according to the following mass percentages: 80% Stellite6 powder (95%–100% sphericity); 8% carbon nanotube powder (purity >99%, inner diameter 3–5 nm, outer diameter 8–15 nm, length 8–14 nm); and 15% B4C ceramic powder. The sum of the mass percentages of the above components is 100%.

[0052] Step 2: After the composite powder has been prepared, mix it evenly and place it in a vacuum tube furnace for heating and drying, then cool it to room temperature. 99.9% Ar gas is introduced into the vacuum tube furnace, the drying temperature is 120℃, and the drying time is 60 minutes.

[0053] Step 3: Pour the dried composite powder into a planetary ball mill without adding grinding balls, and ball mill at 300 rpm for 1 hour. Stop the mill for 15 minutes, then ball mill for another hour. The protective gas is 99.9% Ar gas. Then pour the mixed powder onto the assembled sieve, vibrating screen, and sieve bottom. Start the vibrating screen for sieving for 10 minutes, selecting fiber-modified reinforcing phase laser cladding composite powder with a diameter of 15–50 μm.

[0054] The fiber-modified reinforced phase laser cladding composite powder was placed in the powder feeding device of the laser cladding machine, and arc cladding was performed on 45 steel and then cooled. The laser cladding process parameters were: scanning speed of 5 mm / s, laser power of 1050 W, spot diameter of 4 mm, and both the protective gas and the powder feeding gas were 99.9% Ar gas. The target corrosion-resistant and friction-resistant wind turbine blade bearing surface modification structure was obtained.

[0055] The wear-resistant cladding layer was subjected to room temperature dry tribology tests under non-vacuum conditions. The friction mode was linear reciprocating motion, the load was 15 N, the friction pair material was Si3N4 ceramic balls, and the friction time was 30 min. Figure 1The wear resistance of the unmodified Q235 steel is 65.3 mg, while that of the wear-resistant cladding is 8.7 mg. Wear resistance directly reflects the degree of friction of the material; lower wear resistance indicates better abrasion resistance. The wear-resistant cladding shows a significant improvement in abrasion resistance compared to the substrate. The microhardness of the wear-resistant cladding was measured under a load of 1000 N for 15 seconds at a measurement interval of 0.10 mm. The measurement results are as follows. Figure 4 The wear-resistant cladding layer shown exhibits relatively small differences in hardness distribution across different parts, and its hardness is significantly higher than that of the substrate. The microstructure of the wear-resistant cladding layer is as follows: Figure 7 The structure shown is mainly composed of columnar crystals, with a fine, uniform, and dense structure. There are no obvious defects such as pores or cracks at the interface, which shows that the wear-resistant cladding layer and the matrix are well bonded. Combined with friction and wear test, microhardness test and metallographic analysis at the interface, the wear-resistant cladding layer of the present invention has excellent friction resistance. The reinforcing phase of the prepared wear-resistant cladding layer is uniformly distributed and there is no large regional difference in mechanical properties.

[0056] The embodiments described above merely illustrate specific implementations of the present invention, and while the descriptions are detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers, characterized in that, The mixture comprises 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 10-25% carbide ceramic powder, with the sum of the mass percentages of the above components being 100%; the cobalt-based alloy powder is Stellite6 with a sphericity of 95%-100%; the carbon nanotube powder has a purity >99%, an inner diameter of 3-5 nm, an outer diameter of 8-15 nm, and a length of 8-14 nm; the carbide ceramic powder is either B4C or TiC.

2. The method for preparing fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers according to claim 1, characterized in that, Specifically, the following steps are included: Step 1: Weigh out 70-80% cobalt-based alloy powder, 5-15% carbon nanotube powder, and 10-25% carbide ceramic powder by mass percentage, with the sum of the mass percentages of the above components being 100%. Step 2: Mix the composite powder prepared in Step 1 evenly and place it in a vacuum tube furnace for drying. 99.9% Ar gas is introduced into the tube furnace. The drying temperature is 110℃~120℃ and the drying time is 30min~60min. After drying, keep it at the heat and then cool it to room temperature. Step 3: Mix the composite powder dried in Step 2, and then perform particle size sieving to obtain fiber-modified reinforced phase laser cladding composite powder. The specific procedure for the mixing process is as follows: the composite powder obtained in step 2 is poured into a planetary ball mill without adding grinding balls, the speed is 200~300 rpm, the milling time is 1 hour, the milling interval is 15 minutes, and then the milling time is 1 hour. The protective gas is 99.9% Ar gas.

3. The method for preparing fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers according to claim 2, characterized in that, The specific procedure for particle size sieving in step 3 is as follows: Pour the mixed composite powder onto the assembled screen, vibrating screen and screen bottom, start the vibrating screen for sieving, and sieve for 5-10 minutes to screen out composite powder with a particle size of 15-50μm.

4. The application of fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layer according to claim 1 in laser cladding, wherein the fiber-modified reinforced phase laser cladding composite powder is placed in the powder feeding device of the laser cladding machine, laser cladding is performed on low carbon steel and cooled, thereby obtaining the desired wear-resistant cladding layer.

5. The application of the fiber-modified reinforced phase laser cladding composite powder for wear-resistant cladding layers according to claim 4 in laser cladding, characterized in that, The laser cladding process parameters are as follows: scanning speed is 4mm / s ~ 5mm / s, laser power is 850W ~ 1050W, spot diameter is 4mm, and both the protective gas and the powder feeding gas are 99.9% Ar gas.

Citation Information

Patent Citations

  • Preparation method for wear-resistant and corrosion-resistant composite coating layer

    CN108611636A