Nitrocellulose membranes, their preparation methods and applications

By controlling the fiber knots and fiber diameter of the nitrocellulose membrane and optimizing the membrane's structural parameters, the membrane clogging problem was solved, the sensitivity and signal-to-noise ratio of protein detection were improved, and accurate detection at high crawling speeds was achieved.

CN117861461BActive Publication Date: 2026-11-17HANGZHOU COBETTER FILTRATION EQUIPMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311742205.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-17
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

Existing nitrocellulose membranes suffer from membrane clogging due to their large porosity and pore size in protein detection, which affects detection accuracy and signal-to-noise ratio, especially when the protein molecular weight is large or the chromogenic reagent particle size is large.

Method used

By controlling the fiber nodes and fiber diameter of the nitrocellulose membrane, limiting the relationship between node distribution density, average diameter and membrane thickness, the specific surface area and porosity of the membrane are optimized. A phase separation method is used to prepare the membrane to form a uniform network structure, ensuring good flow performance and separation effect.

Benefits of technology

This technology reduces membrane clogging under high crawling speeds, improves detection sensitivity and signal-to-noise ratio, reduces background noise, and ensures the accuracy of protein detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117861461B_ABST
    Figure CN117861461B_ABST
Patent Text Reader

Abstract

This application relates to filtration materials, specifically to nitrocellulose membranes, their preparation methods, and applications. The nitrocellulose membrane is formed from nitrocellulose fibers, which interweave and cross-link to form a network structure, creating internal flow channels for liquid passage. The membrane is characterized by a thickness of 100–130 μm, the presence of nodes on the fibers, a node average diameter to fiber average diameter ratio of 1.5–2.5, and a node distribution density of 35–70 nodes / (50 μm) on the outer surface of the nitrocellulose membrane. 2 The above technical solution reduces the non-specific adsorption of nitrocellulose membranes and improves the separation effect of nitrocellulose membranes on proteins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to materials for filtration, specifically to nitrocellulose membranes and their preparation methods and applications. Background Technology

[0002] Immunochromatography is an important method for protein detection. It involves labeling a chromogenic reagent with a binding antigen and immobilizing the labeled antigen on a chromatographic membrane. A detection antibody is immobilized on the detection line. As the protein-binding antigen-chromogenic reagent-labeled antibody binding structure moves across the membrane, the detection antibody on the detection line binds to the target protein, causing a color reaction on the detection line. The labeled antibody-chromogenic reagent-binding antigen binding structure that does not bind to the target protein continues to the control line, where the antigen for binding the labeled antibody is immobilized. This keeps the system on the control line, producing a color reaction there. Based on this process, samples that show color only on the control line are negative, while samples that show color on both the control and detection lines are positive. Commonly used chromogenic reagents include latex microspheres, polystyrene microspheres, and colloidal gold.

[0003] The properties of chromatographic membranes have a significant impact on the process of chromogenic immunochromatography. Among them, nitrocellulose membranes are a commonly used chromatographic membrane, which has the characteristics of low background, high signal-to-noise ratio, simple use and easy sealing, and is widely used in the field of protein chromatography detection.

[0004] For nitrocellulose membranes, the migration speed of proteins in the system is closely related to the membrane's porosity and pore size. Generally, nitrocellulose membranes with larger porosity and pore diameters exhibit higher migration speeds and can also allow larger particle sizes of chromogenic agents to pass through. However, when the protein molecular weight is large or the chromogenic agent particle size is large, membrane blockage can easily occur in the pores, leading to inaccurate chromatography results, higher noise levels, darker background color, and jagged edges in the streaks. Summary of the Invention

[0005] To reduce non-specific adsorption of the membrane and improve the separation effect of nitrocellulose membrane for proteins, this application provides a nitrocellulose membrane, its preparation method and application. When used for protein detection at high crawling speeds, it improves detection sensitivity, reduces background color, and reduces membrane clogging.

[0006] First, the nitrocellulose membrane provided in this application is formed by nitrocellulose fibers, which interweave to form a mesh structure and create flow channels for liquid to pass through. The fibers have nodes, and the ratio of the average diameter of the nodes to the average diameter of the fibers is 1.5 to 2.5. On the outer surface of the nitrocellulose membrane, the node distribution density is 35 to 70 nodes / (50 μm). 2.

[0007] Cellulose membranes are typically prepared using methods such as phase separation. Small nodules form on the surface fibers, generally formed by the aggregation of nitrocellulose in solution. These nodules contain complex molecular chain entanglements, but can be viewed as a small sphere attached to the fibers. They significantly influence the flow properties of the liquid and the retention performance of the material. Due to the generally rapid nucleation and precipitation rates at the surface of the phase-separated nitrocellulose membrane, more fiber nodules form on its surface.

[0008] In this application, the number and density of fiber nodes on the nitrocellulose membrane surface must be controlled within a certain range. First, the nodes should not be dense and small, nor should their diameter be too large. Small nodes will fill the pores of the nitrocellulose membrane, further encroaching on the original pore space and causing the strips to turn white. Simultaneously, excessively large nodes will lead to uneven resistance to material movement within the membrane. Proteins will experience greater resistance from these nodes, and in some cases, the node surface may accumulate charge, affecting the electrostatic balance of the entire membrane and causing proteins to be adsorbed onto the nitrocellulose membrane.

[0009] Preferably, the distribution density of the nodes, the average diameter of the nodes, and the average thickness of the nitrocellulose membrane have the following relationship: N·D1 2 =L·K1; where N is the node distribution density, D1 is the average node diameter, L is the thickness of the nitrocellulose membrane, and K1 is a constant with a value ranging from 12000 to 25000 nodes / μm.

[0010] In the above scheme, a larger membrane thickness corresponds to a higher node distribution density. Using the formula above, the node distribution density corresponding to membranes of different thicknesses can be approximately calculated, or the thickness of the prepared membrane can be limited by a specific node distribution density. Specifically, a larger membrane thickness can accommodate a larger average node diameter and node distribution density. With a larger membrane thickness, a larger internal space can be generated inside the membrane, and the influence of the outer layer on the interior is smaller. Therefore, the area with significant internal fibrosis is larger, resulting in a greater overall loading capacity. Proteins can have a better passage rate inside the cellulose membrane, so more proteins will flow through the internal space of the nitrocellulose membrane. Therefore, even with a large fiber node diameter and fiber distribution density, good climbing speed and separation effect can still be achieved.

[0011] Preferably, the average diameter between the fiber average diameter D2 and the average SEM pore size R1 of the nitrocellulose membrane has the following relationship:

[0012]

[0013] Where K2 is a constant, its value ranges from 0.295 to 0.445 μm. 0.5 .

[0014] In the above scheme, the fiber diameter is directly proportional to the square root of the average pore size of the outer surface, and inversely proportional to the square root of the average pore size. This parameter is controlled within a certain range, which means that the smaller the overall pore size in the surface area or near the surface of the nitrocellulose membrane, the finer the fiber structure it should have, and the greater the corresponding porosity. Therefore, with a specific fiber diameter, the refinement of surface pores requires an increase in overall porosity to maintain a good climbing speed and a good separation effect.

[0015] Preferably, the average diameter of the nodes ranges from 3.5 to 5.2 μm, and the average diameter of the fibers ranges from 1.3 to 2.3 μm.

[0016] In the above scheme, the average diameter of the fiber nodes is limited to a certain range, which in turn limits the average diameter of the fibers. Within this range, the efficiency of protein passage can be satisfied, the obstruction of fibers and fiber nodes to proteins can be reduced, and at the same time, it can play a good supporting role for the flow channel, so that the cellulose membrane is not easy to collapse during use, the membrane pores maintain good performance, and thus maintains a good creep rate and loading level.

[0017] Preferably, the average SEM pore size of the nitrocellulose membrane is 20–35 μm, and the specific surface area of ​​the nitrocellulose membrane is 40–80%.

[0018] In the above scheme, the specific surface area of ​​the nitrocellulose membrane is further limited. When used for protein chromatography, the larger the specific surface area of ​​the nitrocellulose membrane, the stronger its ability to adsorb proteins, and the easier it is to cause a slowdown in the flow rate inside the membrane. Therefore, in this application, the specific surface area of ​​the membrane should be controlled within a certain range. An excessively large specific surface area of ​​the membrane will cause the adsorption performance of proteins in the region to be too strong, which will lead to increased noise and reduced sensitivity. On the other hand, an excessively small specific surface area of ​​the membrane will also lead to insufficient membrane loading, and the amount of chromogenic reagent and detection antibody that can be fixed is small, resulting in a high detection limit of the detection line and the quality control line.

[0019] Preferably, the ratio of the surface node coverage area of ​​the nitrocellulose membrane to the cross-sectional pore area of ​​the nitrocellulose membrane is not greater than 0.48.

[0020] For high-speed nitrocellulose membrane systems, as the liquid rapidly passes through the cellulose membrane, the proteins and other macromolecules are affected by the intramembrane nodes, resulting in resistance. In the cross-sectional SEM of the membrane, there are laterally extending flow channels for the liquid and proteins to pass through. The nodes protruding from the fibers cover the pores of the cross-section, thus generating flow resistance. This causes the proteins to flow at different velocities in different regions, resulting in wider and whiter bands. By limiting the area of ​​membrane pores covered by nodes, the membrane achieves lower flow resistance, greater capacity, and more regular bands while maintaining a similar pore area ratio.

[0021] Preferably, the ratio between the average length of the pore in the horizontal direction and the average diameter of the nodes on the nitrocellulose membrane surface is 1.5 to 3.5.

[0022] In cross-section, the horizontal pore length of a filter membrane represents the degree to which liquid can flow smoothly. During the flow of liquid through a nitrocellulose membrane, the liquid flows along the horizontal fibers and is guided by the nodes. Therefore, a good flow effect can be achieved when the ratio of the average horizontal pore length to the average node diameter is within the specified range. If the average horizontal pore length is too large, the surface may have lower flow resistance, but the internal support effect will be poor, making the membrane prone to collapse during use and thus causing membrane blockage.

[0023] Preferably, the outer surface node coverage area ratio P1 and outer surface pore area ratio P2, as well as the node average diameter D1 and fiber average diameter D2, have the following relationship: (P2 / P1)∶(D1 / D2)=0.1~0.2.

[0024] For nitrocellulose membranes with higher creep rates, the pore area ratio on the outer surface is larger. The ratio between the node coverage area and the pore area reflects the available flow channels for liquid flow; the larger this ratio, the higher the available creep rate. Given a specific ratio between the node coverage area and the pore area, the square of the node diameter is inversely proportional to the available flow rate. This is mainly because the cross-sectional area of ​​the node in the flow channel is positively correlated with the resistance the node exerts on the liquid; the larger the node diameter, the lower the applicable creep rate.

[0025] Preferably, the ratio of the outer surface node coverage area P1 to the outer surface porosity P2 is in the range of 0.25 to 0.35.

[0026] In the above scheme, the nodes should not cover too large a surface area in the system, otherwise it will lead to excessive resistance to liquid flow and uneven spatial distribution in the system, which will result in phenomena such as whitening and breakage of the strips.

[0027] Based on the above, this application also provides the following technical solution for preparing the corresponding nitrocellulose membrane:

[0028] The preparation method of nitrocellulose membrane includes the following steps:

[0029] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution, wherein solvent A comprises a combination of ester or ketone organic solvents and alcohol solvents, and the mass fraction of nitrocellulose in the casting solution is 20-50%.

[0030] S2. Apply the casting solution to the substrate. In this step, the substrate is first pre-wetted by solvent A.

[0031] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0032] S4. Immerse the first intermediate product in a water-based coagulation bath and perform phase separation treatment to obtain the second intermediate product.

[0033] S5. The second intermediate product is washed and dried to complete the preparation.

[0034] The thickness of the nitrocellulose membrane is 100–130 μm.

[0035] In the above scheme, the substrate is first wetted with solvent A before preparation, followed by a two-step process of vapor phase separation and liquid phase separation. The vapor phase separation process can control the nucleation step of nitrocellulose. In this process, a combination of low-polarity solvents such as ketones or esters and high-polarity solvents such as alcohols is used as the solvent system. By utilizing the difference in polarity, the stability of the system during the vapor phase separation process is improved. During the vapor phase separation process, after nucleation within the system, nitrocellulose tends to continue growing on the nucleus surface rather than forming new nuclei. This prevents the formation of excessively small and fragmented nuclei in the system, resulting in a more uniform overall structure and making it easier to control the formation of nodes in the surface region.

[0036] Preferably, in step S1, the mass ratio of the casting solution is as follows: nitrocellulose: 20-30 parts, surfactant: 0.5-3 parts, pore-forming agent: 0.1-3 parts, solvent A: 60 parts.

[0037] In the above scheme, a casting solution with a high concentration of nitrocellulose was used. The nodal structure and fiber diameter formed on the surface of the casting solution within this concentration range can just meet the parameters corresponding to this application. However, if the concentration is too high, the nitrocellulose membrane will easily form a denser skin layer on the surface, which will have an adverse effect on the color development. On the other hand, if the density is too low, the fiberization step in the system will be too slow, forming a finer fiber structure and generating finely distributed porous fibers, which will increase the resistance to liquid flow.

[0038] Preferably, solvent A is a combination of branched alkyl ketones or cycloalkyl ketones and monohydric fatty alcohols.

[0039] The solvent A system described above has good polarity, which can fully accommodate the dispersion system of nitrocellulose, and has a good precipitation rate during the phase separation process. Especially when vapor phase separation is carried out in step S3, a system with moderate node particle size and node distribution density can be formed, thereby improving the quality of the prepared nitrocellulose membrane.

[0040] More preferably, solvent A is a combination of cyclopentanone or cyclohexanone and a fatty alcohol, wherein the mass fraction of the fatty alcohol is 25-50%.

[0041] Within this range, the prepared nitrocellulose membrane has better properties and is easier to control in terms of the number and size of nodes.

[0042] Preferably, in step S3, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 30-60% and an isopropanol partial pressure of 0.2-5%. More preferably, in step S3, the temperature is 30-50°C, the air velocity is 0.5-5 m / s, and the contact time is 45-120 s.

[0043] In the above scheme, by adding a certain amount of isopropanol to the steam, the phase separation in this step will not be too fast, which would lead to excessive surface precipitation. At the same time, isopropanol can make the relationship between the generated node diameter and fiber diameter more stable.

[0044] Preferably, in step S4, the temperature is controlled at 20–50°C and the processing time is 30–300 seconds.

[0045] The nitrocellulose membrane prepared within the above range has just the right porosity and specific surface area, stable structure, and can generate good creep rate, as well as good sensitivity and signal-to-noise ratio.

[0046] This application also relates to protein chromatography test strips prepared using the above-mentioned nitrocellulose membrane or nitrocellulose membrane prepared by the above method as raw materials.

[0047] In summary, this application provides a nitrocellulose membrane and a series of methods for preparing the nitrocellulose membrane. When applied to the field of chromogenic protein immunoassay, it can still achieve a high creep rate even when the protein molecular weight is large or the chromogenic particle size is large, and it is not prone to membrane clogging, thereby reducing background noise and improving the signal-to-noise ratio. This makes the nitrocellulose membrane more sensitive when used for protein detection. Attached Figure Description

[0048] Figure 1 This is a schematic SEM image of the nitrocellulose membrane surface in Example 1;

[0049] Figure 2 This is a schematic SEM image of the cross-section of the nitrocellulose membrane in Example 1;

[0050] Figure 3 This is a schematic SEM image of the nitrocellulose membrane surface in Example 8;

[0051] Figure 4 This is a schematic diagram comparing the homogeneity of nitrocellulose membrane chromatography in Examples 1 and 8; the areas indicated by the arrows in the diagram are the underlined areas.

[0052] Figure 5 This is a crisscross diagram of the nitrocellulose membranes in Examples 9 and 10. Detailed Implementation

[0053] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0054] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0055] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0056] Nitrocellulose membranes are commonly used as colorimetric reagents in protein chromatography, and the modification and expansion of their properties have always been a research focus in related fields. Currently, there is no clear research plan for the different applications of nitrocellulose chromatographic membranes in various fields.

[0057] Nitrocellulose membranes are typically prepared by a phase separation method, which can form a relatively uniform system. Since the outer regions in the thickness direction play a major role in color development, and the phase separation method can easily adjust the structure of the surface region of the nitrocellulose membrane, this application mainly uses the phase separation method to prepare the target nitrocellulose membrane. However, it should be noted that other preparation methods can also prepare nitrocellulose membranes with similar physical and chemical properties to those in the following examples.

[0058] In the following examples, the properties of various parameters in the nitrocellulose membrane were determined by the following methods:

[0059] The average pore size on the surface of nitrocellulose membranes, or the average pore size of the cross-section, or the number of nodes, can all be determined by characterizing the membrane structure using a scanning electron microscope (SEM), followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or manually. In actual measurement, the membrane surface can be characterized first using an electron microscope to obtain the corresponding SEM image. Since the pores on the membrane surface are roughly uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation. Then, use the corresponding computer software or manually measure the diameter of all holes on this area, and then calculate to obtain the average diameter of the holes on this surface.

[0060] The areas of nodes and holes can be calculated in the same way. This can be done by manually dividing the approximate hole and node regions and then analyzing and calculating them using a computer, or by using a grid method. Similarly, fiber length can be calculated by manually marking the fiber trajectory and then using a computer.

[0061] It should be noted that those skilled in the art can also obtain the above parameters through other measurement methods, and the above measurement methods are for reference only.

[0062] Examples 1-25 involve different nitrocellulose membranes and corresponding protein chromatography test strips. The SEM image of the nitrocellulose membrane surface in Example 1 is shown below. Figure 1 As shown, the cross-sectional SEM image is as follows. Figure 2 As shown.

[0063] Nitrocellulose membranes are formed from nitrocellulose fibers, which are precipitated using a phase separation method to form an interwoven network structure with internal channels for liquid passage. Figure 1As can be seen, the nitrocellulose membrane in this embodiment has nodes on its surface.

[0064] For Examples 1-25, the microscopic parameters of the nitrocellulose membranes prepared are shown in Table 1.

[0065]

[0066]

[0067] Where K1 = node distribution density N · average node diameter D1 2 / film thickness L, in units of / μm.

[0068]

[0069] K3 represents the surface knot coverage area ratio P1 and surface hole area ratio P2, and the average knot diameter D1 and average fiber diameter D2 have the following relationship (P2 / P1)∶(D1 / D2).

[0070] In the table above, the statistical method for node distribution density involves dividing the region and counting the number of nodes with clear outlines. If a node does not have a clear outline, for example, in... Figure 1 The area marked by circle 1 has 1 node and is not included in the statistics of the average node diameter. Area A shows a clustered node structure. In this area, the clustered nodes are divided into each node according to the outermost node structure, as shown in circle 2. When calculating the average node diameter, only the nodes in circle 2 are counted. However, when calculating the coverage area of ​​the outer surface nodes, all clustered nodes in area A are included in the statistics.

[0071] It is worth noting that in the figure, the clustered node structure in region A is actually caused by the stacking of some nodes in the thickness direction, which will show the clustering phenomenon in the microscopic image. Therefore, only the node structure located on the outermost side is counted.

[0072] When calculating the average SEM pore size and pore area fraction of the membrane, only the pore size of the outermost pores under the SEM microscope is counted, i.e., the outermost ring of fiber structure in the image, for example, in... Figure 1 In the diagram, the circles shown in circle 3 can be included in the statistics, while the circles formed by circle 4 are not included in the statistics.

[0073] The statistical methods for the cross-sectional area ratio covered by nodes and the cross-sectional porosity are the same as those for the outer surface.

[0074] Specific surface area ratio (SAR) is obtained by measuring the specific surface area of ​​the system and then dividing it by the membrane area. The specific surface area of ​​nitrocellulose membranes was determined using the BET surface area assay.

[0075] The method for preparing the nitrocellulose membrane in Example 1 is as follows:

[0076] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0077] Solvent A: 60 parts;

[0078] Nitrocellulose: 20 parts;

[0079] Surfactant: 1 part;

[0080] Pore-forming agent: 2 parts;

[0081] Specifically, solvent A is a mixed solution of 70% cyclopentanone and 30% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0082] The surfactant used is polyethylene glycol octylphenyl ether;

[0083] The porogen is PEG800.

[0084] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution to the substrate with a coating thickness of 500μm.

[0085] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0086] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 50% and an isopropanol partial pressure of 3.2%; the temperature is 45°C, the air velocity is 2.8 m / s, and the contact time is 60 s.

[0087] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 180s.

[0088] It should be noted that electrolytes such as sodium chloride or pH adjusters such as sodium hydroxide can also be added to water-based coagulation baths.

[0089] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0090] The preparation method of the nitrocellulose membrane in Example 2 is as follows:

[0091] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0092] Solvent A: 45 parts;

[0093] Nitrocellulose: 45 parts;

[0094] Surfactant: 1 part;

[0095] Pore-forming agent: 1.8 parts;

[0096] Specifically, solvent A is a mixed solution of 70% cyclopentanone and 30% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0097] The surfactant used is polyethylene glycol octylphenyl ether;

[0098] The porogen is PEG800.

[0099] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0100] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0101] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 48% and an isopropanol partial pressure of 3.2%; the temperature is 50°C, the air velocity is 1.0 m / s, and the contact time is 120 s.

[0102] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 35℃, and the immersion time is 150s.

[0103] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0104] The preparation method of the nitrocellulose membrane in Example 3 is as follows:

[0105] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0106] Solvent A: 60 parts;

[0107] Nitrocellulose: 20 parts;

[0108] Surfactant: 1 part;

[0109] Pore-forming agent: 2.3 parts;

[0110] Specifically, solvent A is a mixed solution of 70% cyclopentanone and 30% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0111] The surfactant used is polyethylene glycol octylphenyl ether;

[0112] The porogen is PEG800.

[0113] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0114] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0115] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 5%; the temperature is 50°C, the air velocity is 5.0 m / s, and the contact time is 55 s.

[0116] S4. The first intermediate product is immersed in a water-based coagulation bath and subjected to phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 240s.

[0117] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0118] The method for preparing the nitrocellulose membrane in Example 4 is as follows:

[0119] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0120] Solvent A: 80 parts;

[0121] Nitrocellulose: 20 parts;

[0122] Surfactant: 1.5 parts;

[0123] Pore-forming agent: 2.5 parts;

[0124] Specifically, solvent A is a mixed solution of 70% cyclopentanone and 30% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~107 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0125] The surfactant used is polyethylene glycol octylphenyl ether;

[0126] The porogen is PEG800.

[0127] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0128] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0129] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 50% and an isopropanol partial pressure of 0.5%; the temperature is 30°C, the air velocity is 4.6 m / s, and the contact time is 120 s.

[0130] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 180s.

[0131] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0132] The method for preparing the nitrocellulose membrane in Example 5 is as follows:

[0133] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0134] Solvent A: 60 parts;

[0135] Nitrocellulose: 20 parts;

[0136] Surfactant: 1 part;

[0137] Pore-forming agent: 1.3 parts;

[0138] Specifically, solvent A is a mixed solution of 60% cyclopentanone and 40% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0139] The surfactant used is polyethylene glycol octylphenyl ether;

[0140] The porogen is PEG800.

[0141] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0142] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0143] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 50% and an isopropanol partial pressure of 3.2%; the temperature is 50°C, the air velocity is 1.1 m / s, and the contact time is 95 s.

[0144] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 180s.

[0145] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0146] The method for preparing the nitrocellulose membrane in Example 6 is as follows:

[0147] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0148] Solvent A: 50 parts;

[0149] Nitrocellulose: 30 parts;

[0150] Surfactant: 1 part;

[0151] Pore-forming agent: 2 parts;

[0152] Specifically, solvent A is a mixed solution of 50% cyclopentanone and 50% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0153] The surfactant used is polyethylene glycol octylphenyl ether;

[0154] The porogen is PEG800.

[0155] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0156] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0157] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 35% and an isopropanol partial pressure of 5%; the temperature is 30°C, the air flow rate is 0.5 / s, and the contact time is 60s.

[0158] S4. The first intermediate product is immersed in a water-based coagulation bath and subjected to phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 40℃, and the immersion time is 300s.

[0159] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0160] The method for preparing the nitrocellulose membrane in Example 7 is as follows:

[0161] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0162] Solvent A: 60 parts;

[0163] Nitrocellulose: 34 parts;

[0164] Surfactant: 1 part;

[0165] Pore-forming agent: 0.5 parts;

[0166] Specifically, solvent A is a mixed solution of 65% cyclopentanone and 35% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0167] The surfactant used is polyethylene glycol octylphenyl ether;

[0168] The porogen is PEG800.

[0169] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0170] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0171] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 2.4%; the temperature is 50°C, the air velocity is 2.8 m / s, and the contact time is 90 s.

[0172] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 180s.

[0173] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0174] The method for preparing the nitrocellulose membrane in Example 8 is as follows:

[0175] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0176] Solvent A: 60 parts;

[0177] Nitrocellulose: 20 parts;

[0178] Surfactant: 1 part;

[0179] Pore-forming agent: 3 parts;

[0180] Specifically, solvent A is cyclopentanone, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0181] The surfactant used is polyethylene glycol octylphenyl ether;

[0182] The porogen is PEG800.

[0183] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0184] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0185] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 50% and an isopropanol partial pressure of 3.2%; the temperature is 45°C, the air velocity is 2.8 m / s, and the contact time is 60 s.

[0186] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 180s.

[0187] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0188] The method for preparing the nitrocellulose membrane in Example 9 is as follows:

[0189] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0190] Solvent A: 60 parts;

[0191] Nitrocellulose: 30 parts;

[0192] Surfactant: 1 part;

[0193] Pore-forming agent: 1 part;

[0194] Specifically, solvent A is a mixed solution of 80% cyclopentanone and 20% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0195] The surfactant used is polyethylene glycol octylphenyl ether;

[0196] The porogen is PEG800.

[0197] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0198] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0199] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 1.5%; the temperature is 40°C, the air velocity is 4 m / s, and the contact time is 90 s.

[0200] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 300s.

[0201] It should be noted that electrolytes such as sodium chloride or pH adjusters such as sodium hydroxide can also be added to water-based coagulation baths.

[0202] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0203] The method for preparing the nitrocellulose membrane in Example 10 is as follows:

[0204] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0205] Solvent A: 85 parts;

[0206] Nitrocellulose: 12 parts;

[0207] Surfactant: 1 part;

[0208] Pore-forming agent: 2 parts;

[0209] Specifically, solvent A is a mixed solution of 80% cyclopentanone and 20% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0210] The surfactant used is polyethylene glycol octylphenyl ether;

[0211] The porogen is PEG800.

[0212] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0213] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0214] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 45% and an isopropanol partial pressure of 8%; the temperature is 40°C, the air velocity is 4 m / s, and the contact time is 90 s.

[0215] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 35℃, and the immersion time is 300s.

[0216] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0217] The method for preparing the nitrocellulose membrane in Example 11 is as follows:

[0218] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0219] Solvent A: 60 parts;

[0220] Nitrocellulose: 30 parts;

[0221] Surfactant: 1 part;

[0222] Pore-forming agent: 2 parts;

[0223] Specifically, solvent A is a mixed solution of 80% cyclopentanone and 20% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0224] The surfactant used is polyethylene glycol octylphenyl ether;

[0225] The porogen is PEG800.

[0226] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0227] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0228] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 40% and an isopropanol partial pressure of 5%; the temperature is 30°C, the air velocity is 4 m / s, and the contact time is 90 s.

[0229] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 40℃, and the immersion time is 100s.

[0230] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0231] The method for preparing the nitrocellulose membrane in Example 12 is as follows:

[0232] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0233] Solvent A: 60 parts;

[0234] Nitrocellulose: 25 parts;

[0235] Surfactant: 1 part;

[0236] Pore-forming agent: 1.8 parts;

[0237] Specifically, solvent A is cyclopentanone with a mass fraction, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0238] The surfactant used is polyethylene glycol octylphenyl ether;

[0239] The porogen is PEG800.

[0240] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0241] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0242] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water content of 60%, no isopropanol, a temperature of 60°C, an air velocity of 8 m / s, and a contact time of 120 s.

[0243] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 50℃, and the immersion time is 120s.

[0244] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0245] The method for preparing the nitrocellulose membrane in Example 13 is as follows:

[0246] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0247] Solvent A: 60 parts;

[0248] Nitrocellulose: 25 parts;

[0249] Surfactant: 1 part;

[0250] Pore-forming agent: 2.2 parts;

[0251] Specifically, solvent A is a mixed solution of 75% cyclopentanone and 25% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0252] The surfactant used is polyethylene glycol octylphenyl ether;

[0253] The porogen is PEG800.

[0254] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0255] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0256] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 3.5%; the temperature is 45°C, the air velocity is 5 m / s, and the contact time is 45 s.

[0257] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0258] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0259] The method for preparing the nitrocellulose membrane in Example 14 is as follows:

[0260] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0261] Solvent A: 60 parts;

[0262] Nitrocellulose: 30 parts;

[0263] Surfactant: 1 part;

[0264] Pore-forming agent: 1.6 parts;

[0265] Specifically, solvent A is a mixed solution of 60% cyclopentanone and 40% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0266] The surfactant used is polyethylene glycol octylphenyl ether;

[0267] The porogen is PEG800.

[0268] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0269] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0270] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 0.9%; the temperature is 40°C, the air velocity is 3.0 m / s, and the contact time is 80 s.

[0271] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0272] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0273] The method for preparing the nitrocellulose membrane in Example 15 is as follows:

[0274] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0275] Solvent A: 60 parts;

[0276] Nitrocellulose: 20 parts;

[0277] Surfactant: 1 part;

[0278] Pore-forming agent: 1.5 parts;

[0279] Specifically, solvent A is a mixed solution of 50% cyclopentanone and 50% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0280] The surfactant used is polyethylene glycol octylphenyl ether;

[0281] The porogen is PEG800.

[0282] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0283] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0284] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 2.5%; the temperature is 50°C, the air velocity is 1.20 m / s, and the contact time is 60 s.

[0285] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0286] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0287] The method for preparing the nitrocellulose membrane in Example 16 is as follows:

[0288] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0289] Solvent A: 60 parts;

[0290] Nitrocellulose: 30 parts;

[0291] Surfactant: 1 part;

[0292] Pore-forming agent: 1.6 parts;

[0293] Specifically, solvent A is a mixed solution of 75% cyclopentanone and 50% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0294] The surfactant used is polyethylene glycol octylphenyl ether;

[0295] The porogen is PEG800.

[0296] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0297] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0298] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 0.9%; the temperature is 45°C, the air velocity is 3.0 m / s, and the contact time is 80 s.

[0299] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0300] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0301] The method for preparing the nitrocellulose membrane in Example 17 is as follows:

[0302] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0303] Solvent A: 60 parts;

[0304] Nitrocellulose: 20 parts;

[0305] Surfactant: 1 part;

[0306] Pore-forming agent: 3 parts;

[0307] Specifically, solvent A is a mixed solution of 75% cyclopentanone and 25% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0308] The surfactant used is polyethylene glycol octylphenyl ether;

[0309] The porogen is PEG800.

[0310] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0311] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0312] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 0.2%; the temperature is 40°C, the air velocity is 1.8 m / s, and the contact time is 120 s.

[0313] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 50℃, and the immersion time is 120s.

[0314] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0315] The method for preparing the nitrocellulose membrane in Example 18 is as follows:

[0316] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0317] Solvent A: 60 parts;

[0318] Nitrocellulose: 23 parts;

[0319] Surfactant: 1 part;

[0320] Pore-forming agent: 1.5 parts;

[0321] Specifically, solvent A is a mixed solution of 75% cyclopentanone and 50% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0322] The surfactant used is polyethylene glycol octylphenyl ether;

[0323] The porogen is PEG800.

[0324] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0325] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0326] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 58% and an isopropanol partial pressure of 0.9%; the temperature is 30°C, the air velocity is 3.0 m / s, and the contact time is 80 s.

[0327] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0328] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0329] The method for preparing the nitrocellulose membrane in Example 19 is as follows:

[0330] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0331] Solvent A: 60 parts;

[0332] Nitrocellulose: 21 parts;

[0333] Surfactant: 1 part;

[0334] Pore-forming agent: 1 part;

[0335] Specifically, solvent A is a mixed solution of 50% cyclopentanone and 50% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0336] The surfactant used is polyethylene glycol octylphenyl ether;

[0337] The porogen is PEG800.

[0338] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0339] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0340] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 35% and an isopropanol partial pressure of 2.5%; the temperature is 48°C, the air velocity is 4.2 m / s, and the contact time is 100 s.

[0341] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 120s.

[0342] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0343] The method for preparing the nitrocellulose membrane in Example 20 is as follows:

[0344] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0345] Solvent A: 60 parts;

[0346] Nitrocellulose: 30 parts;

[0347] Surfactant: 0.8 parts;

[0348] Pore-forming agent: 1.9 parts;

[0349] Specifically, solvent A is a mixed solution of 90% cyclopentanone and 10% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0350] The surfactant used is polyethylene glycol octylphenyl ether;

[0351] The porogen is PEG800.

[0352] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0353] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0354] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 70% and an isopropanol partial pressure of 1.2%; the temperature is 40°C, the air velocity is 2.0 m / s, and the contact time is 100 s.

[0355] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 20℃, and the immersion time is 300s.

[0356] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0357] The method for preparing the nitrocellulose membrane in Example 21 is as follows:

[0358] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0359] Solvent A: 60 parts;

[0360] Nitrocellulose: 27 parts;

[0361] Surfactant: 0.8 parts;

[0362] Pore-forming agent: 1.5 parts;

[0363] Specifically, solvent A is a mixed solution of 70% cyclopentanone and 30% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0364] The surfactant used is polyethylene glycol octylphenyl ether;

[0365] The porogen is PEG800.

[0366] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0367] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0368] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 3.5%; the temperature is 50°C, the air velocity is 4.0 m / s, and the contact time is 90 s.

[0369] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 40℃, and the immersion time is 150s.

[0370] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0371] The method for preparing the nitrocellulose membrane in Example 22 is as follows:

[0372] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0373] Solvent A: 60 parts;

[0374] Nitrocellulose: 20 parts;

[0375] Surfactant: 1.5 parts;

[0376] Pore-forming agent: 3 parts;

[0377] Specifically, solvent A is a mixed solution of 60% cyclopentanone and 40% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0378] The surfactant used is polyethylene glycol octylphenyl ether;

[0379] The porogen is PEG800.

[0380] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0381] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0382] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 0.5%; the temperature is 40°C, the air velocity is 2.5 m / s, and the contact time is 120 s.

[0383] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 20℃, and the immersion time is 300s.

[0384] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0385] The method for preparing the nitrocellulose membrane in Example 23 is as follows:

[0386] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0387] Solvent A: 60 parts;

[0388] Nitrocellulose: 30 parts;

[0389] Surfactant: 1 part;

[0390] Pore-forming agent: 2 parts;

[0391] Specifically, solvent A is a mixed solution of 75% cyclopentanone and 25% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0392] The surfactant used is polyethylene glycol octylphenyl ether;

[0393] The porogen is PEG800.

[0394] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0395] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0396] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 3.6%; the temperature is 35°C, the air velocity is 2.5 m / s, and the contact time is 80 s.

[0397] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 260s.

[0398] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0399] The method for preparing the nitrocellulose membrane in Example 24 is as follows:

[0400] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0401] Solvent A: 60 parts;

[0402] Nitrocellulose: 22 parts;

[0403] Surfactant: 1 part;

[0404] Pore-forming agent: 2 parts;

[0405] Specifically, solvent A is a mixed solution of 55% cyclopentanone and 45% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0406] The surfactant used is polyethylene glycol octylphenyl ether;

[0407] The porogen is PEG800.

[0408] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0409] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0410] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 55% and an isopropanol partial pressure of 4.0%; the temperature is 35°C, the air velocity is 4 m / s, and the contact time is 80 s.

[0411] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 30℃, and the immersion time is 260s.

[0412] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0413] The method for preparing the nitrocellulose membrane in Example 25 is as follows:

[0414] S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution. The specific materials in the casting solution are proportioned by mass as follows:

[0415] Solvent A: 60 parts;

[0416] Nitrocellulose: 30 parts;

[0417] Surfactant: 1 part;

[0418] Pore-forming agent: 1 part;

[0419] Specifically, solvent A is a mixed solution of 60% cyclopentanone and 40% ethanol by mass, and nitrocellulose with a number average molecular weight of 10 is selected. 5 ~10 7 The resin system (in this embodiment, the number average molecular weight was determined to be 6 × 10⁻⁶) 5 );

[0420] The surfactant used is polyethylene glycol octylphenyl ether;

[0421] The porogen is PEG800.

[0422] S2. Immerse the substrate in solvent A to wet the surface of the substrate, and then apply the casting solution onto the substrate.

[0423] S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product.

[0424] Specifically, in this step, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 60% and an isopropanol partial pressure of 2.0%; the temperature is 45°C, the air velocity is 1.0 m / s, and the contact time is 120 s.

[0425] S4. The first intermediate product is immersed in a water-based coagulation bath for phase separation treatment to obtain the second intermediate product; wherein the water-based coagulation bath is pure water, the temperature is 20℃, and the immersion time is 240s.

[0426] S5. Wash the second intermediate product with water and ethanol, and dry it to complete the preparation.

[0427] Example 26: The nitrocellulose membranes prepared in Examples 1-25 were used to prepare chromatographic test strips. The specific preparation method includes the following steps:

[0428] 1. The prepared nitrocellulose membrane was streaked to draw the test line and the control line. The control line used goat anti-mouse IgG polyclonal antibody, and the test line used hepatitis B virus monoclonal antibody 1.

[0429] 2. The nitrocellulose membrane after marking is cut and spread and fixed on the substrate material to obtain the reaction zone. In this application, the substrate material is a polyester board.

[0430] 3. A color developer pad is placed at one end of the reaction zone. In this embodiment, the color developer pad uses a microporous membrane structure. In this application, a polypropylene fiber membrane is selected. The preparation method of the color developer pad is as follows:

[0431] The chromogenic reagent solution was adjusted to pH 10 using potassium carbonate. The labeled antibody was added to the solution, and the reaction was carried out with shaking at room temperature. The surface of the chromogenic reagent was then blocked with BSA, followed by centrifugation and washing to obtain the gold-labeled complex. This gold-labeled complex was then sprayed onto a chromogenic reagent pad. In this embodiment, the selected chromogenic reagent particles were latex microspheres with a diameter distribution of 300–400 nm, and the labeled antibody was hepatitis B virus monoclonal antibody 2.

[0432] 4. Lay a sample pad on the outside of the color developer pad. The sample pad is a glass fiber membrane.

[0433] 5. Lay an absorbent pad at the other end of the reaction zone.

[0434] It should be noted that the use of hepatitis B surface antigen in this application is merely for illustrative purposes. In practice, different antigens can also be detected by using different antibodies.

[0435] In this embodiment, different protein chromatography test strips obtained in different embodiments are used, and the test strips are tested. The specific detection method is as follows:

[0436] Prepare a hepatitis B surface antigen buffer solution. The buffer solution is a 10M PBS system. Add 0.05% Triton and an appropriate amount of surfactant to prepare a hepatitis B surface antigen sample with a concentration of 100 ng / mL. Drop the prepared hepatitis B surface antigen buffer solution onto the sample pad for detection.

[0437] In addition to the above, norovirus and adenovirus were added as negative control groups. The concentration of each control group was 1000 ng / ml.

[0438] Various tests were performed on Examples 1 to 25, and the specific test results are shown in Table 2.

[0439] Table 2

[0440]

[0441] Based on the above experimental results, it is evident that the nitrocellulose membrane prepared in this application can achieve negative detection results for both norovirus and adenovirus, and also achieve positive results for hepatitis B surface antigen. The main differences between the various embodiments lie in the uniformity of the chromatography, the sharpness of the streaks, the absence of whitening, and the intensity of the background color. Specifically, in the table above, the streak morphology is observed after streaking the control line and the detection line in step 1. The uniformity of the chromatography is determined by immersing one end of the prepared chromogenic reagent in the buffer chromatography solution to a depth of 3 mm, and then observing the solution climbing. This also determines the climbing speed of the nitrocellulose membrane. The background depth is determined by observing the color change of the reaction area after antigen detection.

[0442] In the above embodiments, Examples 1, 3, 5, 6, 7, 14, 15, 19, 21, and 25 all performed well, with uniform streaking and no obvious defects. The chromatography process was also relatively uniform, belonging to the category of better embodiments. In Examples 4 and 12, the ratio between the node diameter and the fiber diameter was significantly too large. Therefore, compared to the excessively large fiber diameter, the nodes would produce surface inhomogeneity, hindering liquid flow and making the surface more prone to clogging, resulting in a darker color on the surface. In Examples 2 and 13, compared to Example 4, although the ratio between the node and fiber diameters was lower, the excessively large node diameters were generated during the preparation process, which had a significant impact on the chromatographic uniformity of the membrane. Because the areas where the nodes exist would generate greater flow resistance, some areas within the membrane would exhibit poor overall uniformity in terms of streaking velocity, but the impact on the overall line shape and background depth was relatively small.

[0443] Conversely, in Example 18, the ratio of node diameter to fiber diameter is relatively small, which easily leads to the enrichment of node structures on the fiber, forming a locally non-uniform structure. Although the number of nodes is small, their internal distribution is very uneven. The result is that, on the basis of an overall background color, darker color patches are formed in local areas, and the chromatographic uniformity is poor. In Example 24, although the ratio of node diameter to fiber diameter is within the range, the node particle size itself is small. Therefore, its surface is more likely to accumulate charge, which causes some chromogenic agent structures to aggregate or adsorb on the surface of the nodes, resulting in a darker background color. It also easily leads to lighter band colors, reduced sensitivity, false negatives, and other phenomena.

[0444] Although Example 20 has a smaller node diameter compared to Examples 2 and 13, its average pore length is also lower, resulting in excessively high liquid flow resistance in local areas, similar to the phenomena observed in Examples 2 and 13. However, neither of these cases exhibits significant background noise overall. It should be noted that in the case of heterogeneous chromatography, the chromogenic agent bound to the target protein may exhibit different migration rates in different regions, leading to varying reaction times and potentially false negatives. Furthermore, in Example 13, the larger K1 value indicates a higher density of surface nodes. With a thinner membrane, this excessive node density can reduce membrane capacity and cause material dispersion in the scribing area, resulting in whitening on the scribing lines and poor smoothness.

[0445] In Example 8, although the node size met the requirements, the excessive number of nodes in the system not only affected the chromatographic homogeneity but also caused a darker background color. This may be because the excessive number of nodes hindered protein flow during chromatography, leading to membrane blockage and resulting in high non-specific adsorption within the membrane, thus creating significant background noise. Building on this, Example 12, in addition to having a large number of nodes, also had larger node diameters compared to fiber diameters, and a larger node coverage area ratio compared to the porosity area ratio on the outer surface. This resulted in a significant reduction in overall flow rate and also caused greater adsorption internally, making membrane blockage more pronounced than in Example 8, further darkening the background color.

[0446] In Example 9, although the number of nodes is small and non-specific adsorption and film blockage are not easily generated, the fiber diameter is also small. Therefore, the adhesion and retention performance of the material on the surface is poor, and there is a certain whitening of the strips.

[0447] In Example 10, the lower K2 value indicates a lower fiber diameter and a larger average SEM pore size. This results in excessively fast liquid flow on the membrane surface, and uneven scribing in the scribing area. In Examples 16 and 23, the higher K2 value and larger fiber diameter lead to flow imbalance on the surface, resulting in uneven material distribution in the scribing area and a whitening of the stripes. The large fiber diameter also causes non-specific adsorption, which is difficult to wash away due to the smaller pore size, thus creating a background color. In Example 16, the node area occupies a larger portion of the surface area, resulting in a higher K3 value. K3 is the ratio of the surface node coverage area to the surface pore area ratio, and the ratio of the average node diameter to the average fiber diameter. A high K3 value leads to greater overall resistance, reducing creepage speed and increasing the likelihood of membrane clogging. Overall, Example 16 has a larger background color compared to Example 23.

[0448] In Example 11, the larger K3 value, similar to Example 16, leads to a darker background color. Also, in Example 11, the larger coverage area of ​​the nodes compared to the larger surface porosity leads to poorer material aggregation on the membrane surface, making the overall color of the strips lighter and reducing sensitivity.

[0449] In Example 17, unlike Example 13, the K1 value is too small. Although a smaller K1 value means fewer nodes, the nitrocellulose membrane without nodes on its surface actually exhibits poor material binding performance in the scribe lines. Furthermore, despite the smaller number of nodes, there are still fine, fragmented nodes, resulting in poorer control over the creeping speed (specifically, excessively fast creeping speed) and enhanced non-specific adsorption, making it prone to contamination and leading to a darker background color compared to Example 1. A similar situation is observed in Example 22. Although its node size is larger than in Examples 17 and 24, its larger cross-sectional fiber length makes it easier to form uneven flow areas in the horizontal direction during liquid flow. That is, the liquid cannot fully utilize the space within the membrane, and therefore, some antibody and chromogenic components are easily trapped in areas where small nodes aggregate, resulting in a certain background color. This example also leads to excessively fast creeping speed.

[0450] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A nitrocellulose membrane, formed by nitrocellulose fibers interwoven to form a mesh structure, and creating internal channels for liquid passage, characterized in that, The fiber has nodes, and the ratio of the average diameter of the node to the average diameter of the fiber is 1.5 to 2.

5. On the outer surface of the nitrocellulose membrane, the node distribution density is 35 to 70 nodes / (50 μm). 2 ; The distribution density of the nodes, the average diameter of the nodes, and the average thickness of the nitrocellulose membrane have the following relationship: N·D1 2 =L·K1; where N is the node distribution density, D1 is the average node diameter, L is the thickness of the nitrocellulose membrane, and K1 is a constant with a value ranging from 12000 to 25000 nodes / μm.

2. The nitrocellulose membrane according to claim 1, characterized in that, The average diameters of the fiber average diameter D2 and the average SEM pore size R1 of the nitrocellulose membrane have the following relationship: ; Where K2 is a constant, its value ranges from 0.295 to 0.445 μm. 0.5 .

3. The nitrocellulose membrane according to claim 1, characterized in that, The average diameter of the nodes ranges from 3.5 to 5.2 μm, and the average diameter of the fibers ranges from 1.3 to 2.3 μm.

4. The nitrocellulose membrane according to claim 1, characterized in that, The average SEM pore size of the nitrocellulose membrane is 20–35 μm, and the specific surface area of ​​the nitrocellulose membrane is 40–80%.

5. The nitrocellulose membrane according to claim 1, characterized in that, The ratio of the surface node coverage area of ​​the nitrocellulose membrane to the cross-sectional pore area of ​​the nitrocellulose membrane is not greater than 0.

48.

6. The nitrocellulose membrane according to claim 5, characterized in that, On the cross-section of the nitrocellulose membrane, the ratio between the average length of the pores in the horizontal direction and the average diameter of the nodes on the surface of the nitrocellulose membrane is 1.5 to 3.

5.

7. The nitrocellulose membrane according to claim 1, characterized in that, The surface node coverage area ratio P1 and surface hole area ratio P2, as well as the node average diameter D1 and fiber average diameter D2, have the following relationship: (P2 / P1) : (D1 / D2) = 0.1 to 0.

2.

8. The nitrocellulose membrane according to claim 7, characterized in that, The ratio of the surface node coverage area P1 to the surface porosity P2 ranges from 0.25 to 0.

35.

9. A method for preparing a nitrocellulose membrane according to any one of claims 1 to 8, characterized in that, Includes the following steps: S1. Nitrocellulose is dissolved in solvent A to prepare a casting solution, wherein solvent A comprises a combination of ester or ketone organic solvents and alcohol solvents, and the mass fraction of nitrocellulose in the casting solution is 20-50%; S2. Apply the casting solution to the substrate. In this step, the substrate is first pre-wetted by solvent A. S3. The product obtained in step S2 is subjected to a phase separation process by steam separation to obtain the first intermediate product. S4. Immerse the first intermediate product in a water-based coagulation bath and perform phase separation treatment to obtain the second intermediate product. S5. The second intermediate product is washed and dried to complete the preparation. The thickness of the nitrocellulose membrane is 100–130 μm.

10. The method for preparing nitrocellulose membrane according to claim 9, characterized in that: In step S1, the mass ratio of the casting solution is as follows: nitrocellulose: 20-30 parts, surfactant: 0.5-3 parts, pore-forming agent: 0.1-3 parts, solvent A: 60 parts.

11. The method for preparing nitrocellulose membrane according to claim 10, characterized in that, Solvent A is a combination of branched alkyl ketones or cycloalkyl ketones and monohydric fatty alcohols.

12. The method for preparing nitrocellulose membrane according to claim 11, characterized in that, Solvent A is a combination of cyclopentanone or cyclohexanone and fatty alcohol, wherein the mass fraction of the fatty alcohol is 25-50%.

13. The method for preparing a nitrocellulose membrane according to claim 12, characterized in that, In step S3, the steam used is an air system mixed with water and isopropanol, with a water partial pressure of 30-60% and an isopropanol partial pressure of 0.2-5%.

14. The method for preparing a nitrocellulose membrane according to claim 13, characterized in that, In step S3, the temperature is 30–50℃, the air velocity is 0.5–5m / s, and the contact time is 45–120s.

15. The method for preparing a nitrocellulose membrane according to claim 14, characterized in that, In step S4, the temperature is controlled at 20–50°C, and the processing time is 30–300 seconds.

Citation Information

Patent Citations

  • Nitrocellulose microporous membrane and continuous preparation method thereof

    CN114768545A