A clay-like material, its preparation method and application
By synthesizing clay-like materials via a solvothermal method, the problems of stability and composition controllability of natural clay materials have been solved, enabling the application of efficient and low-cost electrocatalysts and expanding their application potential in the field of electrochemistry.
Patent Information
- Application Number
- CN202311597670.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-25
AI Technical Summary
Existing clay materials are limited by the types and proportions of natural mineral elements, making it difficult to achieve stability and controllable composition. The preparation process is energy-intensive and generates pollution from toxic chemical reagents, which affects their application in the field of electrochemistry.
A clay-like material was prepared by a solvothermal method. By adjusting the ratio of tetrahedral and octahedral cations, a dispersion solution was prepared and the pH value was adjusted to synthesize a clay-like material with a layered structure.
This study improved the stability and electrocatalytic activity of clay-like materials, simplified the preparation process, reduced costs, and enhanced the controllability and mass production capabilities of the materials.
Smart Images

Figure CN117865170B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of inorganic materials technology, and in particular to a clay-like material, its preparation method, and its application. Background Technology
[0002] With the rapid growth of the global economy, energy consumption and environmental pollution are two major challenges facing global development. The development and utilization of renewable and clean energy has become one of the greatest challenges to sustainable development in contemporary society, and strengthening the clean energy industry has become an important goal and task of my country's 14th Five-Year Plan. However, renewable energy sources such as solar, wind, and tidal power suffer from intermittency and seasonality, making it difficult to meet daily life needs. Therefore, it is necessary to develop constant and efficient energy storage and conversion systems. Given the wide range of energy applications and high demand, the development of inexpensive and efficient energy materials is crucial.
[0003] Among various energy materials, clay materials possess advantages such as abundant reserves, low price, high ionic conductivity, porous structure, adjustable specific surface area, and good thermal and mechanical stability, demonstrating application potential as electrode, electrolyte, and membrane materials in energy storage and conversion devices. Natural clays share similar elemental compositions and crystal structures, primarily consisting of silicon dioxide and aluminum oxide, with trace amounts of oxides such as sodium, potassium, magnesium, iron, and calcium. The crystal structure of clay minerals is mainly composed of two basic structural units: silicon-oxygen tetrahedra and aluminum-oxygen octahedrons. These tetrahedra and octahedrons are arranged infinitely to form tetrahedral and octahedral layers, respectively. Different forms of stacking and repetition of tetrahedral and octahedral layers result in clay minerals with varying layered structures. A 1:1 structure is formed by stacking one tetrahedral layer and one octahedral layer (e.g., kaolinite, serpentine, hydrotalcite, etc., with the molecular formula generally M3Si2O5(OH)4·nH2O, where M is a divalent metal ion). A 2:1 structure is formed by stacking two tetrahedral layers with an octahedral layer sandwiched between them (e.g., montmorillonite, vermiculite, etc., with the molecular formula generally M3Si4O). 10(OH)₂·nH₂O, where M is a divalent metal ion). Clay materials possess unique crystal structures, microstructures, and excellent physicochemical properties, offering numerous possibilities for their application in energy conversion and storage. However, several unresolved issues remain: the quality of clay minerals from different sources and batches varies significantly, making it difficult to guarantee product quality stability; the transformation from mined natural clay minerals to clay micro / nano materials applicable to energy conversion and storage systems requires extensive purification and modification (e.g., CN104326479A), severely limiting the application of clay materials in the electrochemical field; and the limited variety and proportion of elements in existing clay materials hinders targeted synthesis. Therefore, synthesizing clay-like materials with similar two-dimensional structures to clay minerals will expand the energy material system, simplify material preparation methods, ensure product quality stability, and facilitate their application in the electrochemical field.
[0004] Existing micro / nano-scale clay materials require multiple steps, including selection, wet grinding, heat treatment, acid leaching, and surface modification, which presents problems such as high energy consumption and pollution from toxic chemical reagents. In addition, due to the elemental limitations of natural clay minerals, the prepared clay materials suffer from a limited variety of constituent elements and difficulty in adjusting the component ratios. Summary of the Invention
[0005] Therefore, it is necessary to address the limitations of existing technologies, which are constrained by the elemental limitations of natural clay minerals, resulting in a limited variety of constituent elements and difficulty in adjusting component ratios in the prepared clay materials. This would provide a clay-like material with adjustable composition, controllable structure, and good stability, along with its preparation method and applications.
[0006] To solve the above problems, this application adopts the following technical solution:
[0007] One objective of this application is to provide a method for preparing a clay-like material, comprising the following steps:
[0008] Prepare a first dispersion solution and a second dispersion solution. The first dispersion solution is obtained by mixing a compound containing tetrahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes. The second dispersion solution is obtained by mixing a metal salt or hydroxide containing octahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes.
[0009] Mix the first dispersion solution, the second dispersion solution and the mineralizing agent, adjust the pH of the solution to 7-14, and then disperse by ultrasonication or stirring for 5-40 minutes to obtain a mixed solution.
[0010] The mixed solution was reacted at a constant temperature of 100–200°C for 10–48 hours and then cooled to room temperature.
[0011] The solid product obtained from the reaction was washed and dried to obtain the clay-like material.
[0012] In some embodiments, the tetrahedral cation includes, but is not limited to, one or more of silicon and germanium, and the compound containing the tetrahedral cation includes, but is not limited to, oxides or ionic compounds, wherein the oxide includes at least one of silicon oxide or germanium oxide, and the ionic compound includes at least one of sodium silicate or sodium germanate.
[0013] In some embodiments, the octahedral cation includes, but is not limited to, at least one of alkaline earth metals, transition metals, or rare earth metals. The alkaline earth metals include magnesium, calcium, strontium, or barium. The transition metals include aluminum, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium, ruthenium, cadmium, or indium. The rare earth metals include lanthanum, cerium, or terbium. The metal salts containing octahedral cations include, but are not limited to, chlorides, nitrates, sulfates, and acetates.
[0014] In some embodiments, the mineralizing agent includes, but is not limited to, ammonium chloride, urea, or sodium fluoride; the compound for adjusting the pH of the solution includes, but is not limited to, ammonia, sodium hydroxide, or potassium hydroxide solution.
[0015] In some embodiments, the step of obtaining the clay-like material by washing and drying the solid product obtained from the reaction specifically includes the following steps:
[0016] The solid product was obtained by solid-liquid separation and washed with deionized water until the aqueous solution was neutral. The obtained sample was then dried at 40-80℃ for 12-24 hours to obtain the clay-like material.
[0017] In some embodiments, the solid-liquid separation method includes filtration and centrifugation, and the drying includes vacuum drying, freeze drying, and air drying.
[0018] The second objective of this application is to provide a clay-like material, which is prepared by the aforementioned method for preparing clay-like materials.
[0019] The third objective of this application is to provide an application of the aforementioned clay-like material as an electrocatalyst in the oxygen evolution reaction.
[0020] The present application adopts the above technical solution, and its beneficial effects are as follows:
[0021] The clay-like material and preparation method provided in this application use compounds containing tetrahedral cations, metal salts or hydroxides containing octahedral cations as the main raw materials, and prepares the clay-like material by a solvothermal method. The microstructure and physicochemical properties of the clay-like material are controlled by changing the elemental composition and ratio. The material has a rich elemental composition, controllable structure and composition, and good stability.
[0022] The method for preparing the clay-like material provided in this application is simple, easy to implement, and low in cost. The clay-like material can be prepared in batches using simple and controllable process conditions. The prepared clay-like material is used as an electrocatalyst for alkaline oxygen evolution reaction, and has good electrocatalytic activity and stability. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments of this application or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 A flowchart illustrating the steps of the method for preparing the clay-like material provided in this application embodiment.
[0025] Figure 2 The image shows a scanning electron microscope (SEM) image of the 2:1 type micro / nano clay-like material prepared in Example 1.
[0026] Figure 3 The image shows the X-ray diffraction pattern of the 2:1 type micro / nano clay-like material prepared in Example 1.
[0027] Figure 4 The image shows a scanning electron microscope (SEM) image of the 1:1 micro / nano clay-like material prepared in Example 2.
[0028] Figure 5 The image shows the X-ray diffraction pattern of the 1:1 micro / nano clay-like material prepared in Example 2.
[0029] Figure 6 The linear sweep voltammetry curve of the 1:1 micro / nano clay-like material prepared in Example 2 in 1M potassium hydroxide solution is shown. Detailed Implementation
[0030] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application.
[0031] In the description of this application, it should be understood that the terms "upper", "lower", "horizontal", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0032] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0033] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments.
[0034] Please see Figure 1 This application provides a flowchart of a method for preparing a clay-like material, including steps S110 to S140 below. The implementation of each step is described in detail below.
[0035] Step S110: Prepare a first dispersion solution and a second dispersion solution. The first dispersion solution is obtained by mixing a compound containing tetrahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes. The second dispersion solution is obtained by mixing a metal salt or hydroxide containing octahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes.
[0036] In some embodiments, the tetrahedral cation includes, but is not limited to, one or more of silicon and germanium, and the compound containing the tetrahedral cation includes, but is not limited to, oxides or ionic compounds, wherein the oxide includes at least one of silicon oxide or germanium oxide, and the ionic compound includes at least one of sodium silicate or sodium germanate.
[0037] In some embodiments, the octahedral cation includes, but is not limited to, at least one of alkaline earth metals, transition metals, or rare earth metals. The alkaline earth metals include magnesium, calcium, strontium, or barium. The transition metals include aluminum, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium, ruthenium, cadmium, or indium. The rare earth metals include lanthanum, cerium, or terbium. The metal salts containing octahedral cations include, but are not limited to, chlorides, nitrates, sulfates, and acetates.
[0038] It is understandable that the ratio of tetrahedral cations to octahedral cations in compounds containing tetrahedral cations and metal salts or hydroxides containing octahedral cations can be determined based on the atomic ratio of tetrahedral cations to octahedral cations in the 1:1 or 2:1 clay molecular formula, and can be adjusted as needed in practice.
[0039] In this embodiment, silicon and germanium ions are used as tetrahedral cations in the layered structure of clay, and alkaline earth metal, transition metal or rare earth metal ions are used as octahedral centers. The microstructure and physicochemical properties of the clay-like material are controlled by changing the elemental composition and ratio.
[0040] Step S120: Mix the first dispersion solution, the second dispersion solution and the mineralizing agent and adjust the pH of the solution to 7-14, then sonicate or stir for 5-40 minutes to obtain a mixed solution.
[0041] In this embodiment, the mineralizing agent includes, but is not limited to, ammonium chloride, urea, and sodium fluoride; the compound for adjusting the pH of the solution includes, but is not limited to, ammonia, sodium hydroxide, and potassium hydroxide solution.
[0042] Step S130: The mixed solution is reacted at a constant temperature of 100-200°C for 10-48 hours and then cooled to room temperature.
[0043] Step S140: The solid product obtained from the reaction is washed and dried to obtain the clay-like material.
[0044] In this embodiment, the step of obtaining the clay-like material by washing and drying the solid product obtained from the reaction specifically includes the following steps: separating the solid product by solid-liquid separation, washing it with deionized water until the aqueous solution is neutral, and then drying the obtained sample at 40-80℃ for 12-24 hours to obtain the clay-like material.
[0045] Furthermore, the solid-liquid separation method includes filtration and centrifugation, and the drying includes vacuum drying, freeze drying, and air drying.
[0046] The clay-like material and preparation method provided in this application use compounds containing tetrahedral cations, metal salts or hydroxides containing octahedral cations as the main raw materials, and prepares the clay-like material by a solvothermal method. The microstructure and physicochemical properties of the clay-like material are controlled by changing the elemental composition and ratio. The material has a rich elemental composition, controllable structure and composition, and good stability.
[0047] The method for preparing the clay-like material provided in this application is simple, easy to implement, and low in cost. The clay-like material can be prepared in batches using simple and controllable process conditions. The prepared clay-like material is used as an electrocatalyst for alkaline oxygen evolution reaction, and has good electrocatalytic activity and stability.
[0048] The technical solutions described above in this application will be explained in detail below with reference to specific embodiments.
[0049] Example 1: A method for preparing a 2:1 type clay-like material, which includes the following steps:
[0050] Step 1: Weigh 1.5 mmol of nickel chloride hexahydrate and 2 mmol of sodium silicate, add them to 15 mL of deionized water, and sonicate for 10 minutes;
[0051] Step 2: Stir the sodium silicate aqueous solution from Step 1 at 25°C at a speed of 500 r / min, add the nickel chloride aqueous solution dropwise to the sodium silicate aqueous solution at a rate of 5 mL / min, add 10 mmol of ammonium chloride as a mineralizing agent, add 2 mL of ammonia water, and stir and disperse for 30 minutes.
[0052] Step 3: Transfer the solution obtained in Step 2 to a 50 mL high-pressure reactor and react at 150 °C for 12 hours.
[0053] Step 4: After the reaction vessel has cooled naturally to room temperature, separate the solid product obtained in Step 3 and wash it with deionized water until the aqueous solution is neutral. Place the obtained sample in a vacuum drying oven at 50°C for 12 hours to obtain a 2:1 type micro-nano clay-like material.
[0054] Figure 2 The image shown is a scanning electron microscope image of the 2:1 type micro-nano clay-like material obtained in this embodiment, which shows that the 2:1 type micro-nano clay-like material prepared by the present invention has a regular morphology and a plate-like structure with obvious layered structure.
[0055] Figure 3 The X-ray diffraction comparison diagram of the material prepared in Example 1 shows that the prepared material has obvious diffraction peaks at 2θ of 6.2, 11.9, 19.4, 24.9, 34.5, and 60.5, which are in good agreement with the vermiculite 3M diffraction peaks in the standard database (16-0613), indicating that the generated product is a 2:1 type clay-like material.
[0056] Example 2: A method for preparing a 1:1 clay-like material, comprising the following steps:
[0057] Step 1: Weigh 3 mmol of cobalt chloride hexahydrate and add it to 30 mL of deionized water. Add 0.5 mmol of sodium silicate and 1.5 mmol of sodium germanate to 40 mL of deionized water and sonicate them for 10 minutes respectively.
[0058] Step 2: Stir the sodium silicate and sodium germanate aqueous solution from Step 1 at 25°C at a speed of 500 r / min. Add the cobalt chloride aqueous solution dropwise to the sodium silicate and sodium germanate solution at a rate of 2 mL / min. Add an appropriate amount of 2M sodium hydroxide solution to adjust the pH of the solution system to 13. Stir and disperse for 30 minutes.
[0059] Step 3: Transfer the mixed solution obtained in Step 2 to a 100 mL high-pressure reactor and react at 180 °C for 12 hours.
[0060] Step 4: After the reaction vessel has cooled to room temperature, separate the solid product obtained in step 3 and wash it with deionized water until the aqueous solution is neutral. Place the obtained sample in a vacuum drying oven at 50°C for 12 hours to obtain a 1:1 micro-nano clay-like material.
[0061] Figure 4 The image shown is a scanning electron microscope image of the 1:1 type micro-nano clay-like material obtained in this embodiment. It shows that the 1:1 type micro-nano clay-like material prepared by the present invention has a regular morphology and a distinct layered sheet structure with a thickness of about 20 nm. Figure 5 The image shows a comparison of X-ray diffraction patterns of the 1:1 type micro / nano clay-like material prepared in Example 2. The prepared material exhibits obvious diffraction peaks at 2θ values of 12.2, 19.2, 24.7, 31.4, 35.6, 59.3, and 64.9, which are in good agreement with the diffraction peaks of Mg3Si2O5(OH)4 in the standard database (00-052-1562), indicating that the generated product is a 1:1 type clay-like material. Figure 6 The linear sweep voltammetry curve of the 1:1 type micro / nano clay-like material prepared in Example 2 in 1M potassium hydroxide solution shows that the product exhibits good oxygen evolution performance.
[0062] It is understood that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0063] The above are merely preferred embodiments of this application, and only specifically describe the technical principles of this application. These descriptions are only for explaining the principles of this application and should not be construed as limiting the scope of protection of this application in any way. Based on this explanation, any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application, as well as other specific embodiments of this application that can be conceived by those skilled in the art without creative effort, should be included within the scope of protection of this application.
Claims
1. A method for preparing a clay-like material, characterized in that, Includes the following steps: Prepare a first dispersion solution and a second dispersion solution. The first dispersion solution is obtained by mixing a compound containing tetrahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes. The second dispersion solution is obtained by mixing a metal salt or hydroxide containing octahedral cations with deionized water and then dispersing it by ultrasonication or stirring for 5 to 30 minutes. Mix the first dispersion solution, the second dispersion solution and the mineralizing agent and adjust the pH of the solution to 7-14. Then, disperse the mixture by ultrasonication or stirring for 5-40 minutes to obtain a mixed solution. The mixture was reacted at a constant temperature of 100-200°C for 10-48 hours and then cooled to room temperature. The solid product obtained from the reaction was washed and dried to obtain the clay-like material. The tetrahedral cation includes germanium; the compound containing the tetrahedral cation includes: oxides or ionic compounds; the oxide includes germanium oxide; the ionic compound is sodium germanate; The octahedral cation includes at least one of alkaline earth metals, transition metals, or rare earth metals, wherein the alkaline earth metals include magnesium, calcium, strontium, or barium; the transition metals include copper, zirconium, ruthenium, or cadmium; and the rare earth metals include lanthanum, cerium, or terbium. The metal salts containing octahedral cations include chlorides, nitrates, sulfates, and acetates. The mineralizing agent includes ammonium chloride or sodium fluoride; the compound for adjusting the pH of the solution includes potassium hydroxide solution.
2. The method for preparing a clay-like material according to claim 1, wherein The alkaline earth metals also include magnesium; the transition metals also include aluminum, chromium, manganese, iron, cobalt, nickel, zinc, or indium.
3. The method of preparing a clay mimetic material according to claim 1, wherein The mineralizing agent also includes urea; the compounds for adjusting the pH of the solution also include: ammonia water and sodium hydroxide solution.
4. The method of preparing a clay-mimicking material according to claim 1, wherein The step of obtaining the clay-like material by washing and drying the solid product obtained from the reaction specifically includes the following steps: The solid product was obtained by solid-liquid separation and washed with deionized water until the aqueous solution was neutral. The obtained sample was then dried at 40-80 ℃ for 12-24 hours to obtain the clay-like material.
5. The method of preparing a clay- mimicking material according to claim 4, wherein The solid-liquid separation methods include filtration and centrifugation, and the drying methods include vacuum drying, freeze drying, and air drying.
6. A clay mimetic material, characterized by, It is prepared by the method for preparing clay-like materials according to any one of claims 1 to 5.
7. The application of the clay-like material as described in claim 6 as an electrocatalyst in the oxygen evolution reaction.
Citation Information
Patent Citations
Serpentine nanosheet and preparation method thereof
CN104326479A
Synthetic swelling clay minerals
CN1162295A
Family of microporous indium silicate compositions
US6007790A