Method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step using an inclined single temperature zone synthesis furnace

The one-step method of preparing high-purity selenium, germanium, gallium and barium polycrystalline materials through a tilted single-temperature zone synthesis furnace solves the problems of low purity of BGGSe polycrystalline materials and difficult control of compound ratios, and achieves the synthesis of polycrystalline materials with high purity and high crystallinity. Improved crystal quality and transmittance of single crystal growth.

CN117867637BActive Publication Date: 2024-10-25HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410111971.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2024-10-25
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

The existing synthesis method of BGGSe polycrystalline material results in low purity of the polycrystalline material, which affects the quality of single crystals. Moreover, the synthesis of binary compounds easily introduces oxygen impurities and impurities, making it difficult to control the proportion of compounds and obtain a uniform pure phase.

Method used

High-purity selenium, germanium, gallium and barium polycrystalline materials are prepared using a one-step method in a tilted single-temperature zone synthesis furnace. By grouping materials in an inert atmosphere, molecular pump vacuum processing and hydrogen-oxygen flame sealing are used to control temperature gradients and temperature oscillations to avoid compound decomposition. and segregation to ensure the synthesis of polycrystalline materials in stoichiometric ratios.

Benefits of technology

BaGa2GeSe6 polycrystalline material with high purity and high crystallinity was obtained, which reduced the exchange of raw materials with the external environment, solved the difficulty of controlling the compound ratio and pollution problems, and improved the crystal quality and transmittance of single crystal growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117867637B_ABST
    Figure CN117867637B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing high-purity selenium, germanium, gallium, and barium polycrystalline materials for single crystal growth in one step by using an inclined single-temperature zone synthesis furnace, and relates to a method for preparing polycrystalline materials for single crystal growth. The method aims to solve the technical problem that the BGGSe polycrystalline materials prepared by the existing method for synthesizing BGGSe polycrystalline materials have low purity, thereby affecting the quality of the grown single crystals. The method: 1. Ba source, Ga source, Ge source, and Se source as well as excess Ba source and Ge source are weighed in a glove box with an inert atmosphere according to a stoichiometric ratio; then the material providing a pressure gas atmosphere is weighed; the raw materials are grouped and placed in a cylindrical crucible and a quartz tube, and then the cylindrical crucible is placed in the quartz tube, evacuated, and then inert gas is injected and sealed; and the material is placed in an inclined single-temperature zone tubular furnace for step-by-step reaction to obtain a high-purity selenium, germanium, gallium, and barium polycrystalline material BaGa2GeSe6, whose unit cell structure parameters are consistent with the relevant theoretical values, and each element conforms to the stoichiometric ratio, with high purity, and can be used for single crystal growth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing polycrystalline material for single crystal growth. Background Art

[0002] All-solid-state lasers have the advantages of small size, high beam quality and high power. They have become an important direction of laser technology development and have broad application prospects in important fields such as industry, medicine, national defense and energy. All-solid-state lasers mainly rely on frequency conversion technology based on nonlinear optical crystals to obtain the required laser output band. The intrinsic defects of chalcopyrite crystals (such as AgGaS2, AgGaSe2 and ZnGeP2, etc.) for commercial applications in the infrared band, such as low laser damage threshold and two-photon absorption, limit their application in far-infrared high-power solid-state lasers.

[0003] The article "Crystal growth and characterization of new quaternary chalcogenide nonlinear crystals for the mid-IR: BaGa2GeS6 and BaGa2GeSe6" published in the 2016 issue 6, volume 9, pages 2933-2938 of Optical Materials Express discloses a method for synthesizing BGGSe polycrystalline material and growing single crystals by a "two-step method". The method is to grow single crystals in a vacuum (10 -6 Under the condition of 1000 mbar, the binary phase compounds BaSe, Ga2Se3 and GeSe2 were first synthesized using single elements Ba (99.9%), Ga (99.999%), Ge (99.999%) and Se (99.999%), and then the synthesized binary phase compounds were synthesized at 1000°C for about 24 hours according to the stoichiometric ratio of 1:1:1 to obtain uniform BGGSe polycrystalline material. It was then moved to a vertical Bridgman single crystal growth furnace for crystal growth at a temperature gradient of 10°C / cm and a growth rate of 6mm per day to obtain centimeter-level high-transparency and high-quality BGGSe single crystals. This method uses binary compounds to synthesize polycrystalline. The compounds themselves are easy to absorb water and thus easy to introduce oxygen impurities. In addition, the binary compounds need to be ground, which will also introduce impurities. The low purity of polycrystalline material directly affects the quality of single crystals. Summary of the invention

[0004] The present invention aims to solve the technical problem that the BGGSe polycrystalline material prepared by the existing method for synthesizing BGGSe polycrystalline material has low purity, which in turn affects the quality of the grown single crystal, and provides a method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step using an inclined single temperature zone synthesis furnace.

[0005] The method of the present invention for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step by using an inclined single temperature zone synthesis furnace is carried out according to the following steps:

[0006] 1. In an inert atmosphere glove box, weigh Ba source, Ga source, Ge source and Se source according to the stoichiometric ratio of BaGa2GeSe6; then weigh out 0.01wt.% to 5.00wt.% of Ba source and 0.01wt.% to 10.00wt.% of Ge source to be added; then weigh out a substance providing a pressurized gas atmosphere, wherein the substance providing a pressurized gas atmosphere is 0.01 to 10.00g of elemental selenium, germanium diselenide, red phosphorus or elemental iodine; the Se source is powdered elemental selenium, beaded elemental selenium, barium selenide (BaSe), gallium triselenide (Ga2Se3) or germanium diselenide (GeSe2);

[0007] 2. Divide the weighed materials into two groups, one group is placed in a cylindrical crucible, and the other group is placed in a quartz tube and outside the cylindrical crucible; the materials placed in the cylindrical crucible are Ba source, Ga source, Ge source, compound Se source and excess Ba source and Ge source weighed according to the stoichiometric ratio; the materials placed in the quartz tube and outside the cylindrical crucible are Se source in a single substance state and a material providing a pressurized gas atmosphere;

[0008] Then, the cylindrical crucible is placed in a quartz tube, and the quartz tube is evacuated to a vacuum state by a molecular pump, and then an inert gas is filled into the quartz tube until the reading of the external pressure vacuum gauge reaches -0.010 to -0.015 MPa, and the quartz tube is melted and sealed by a hydrogen-oxygen flame; in order to avoid the decomposition of the selenium-germanium-gallium-barium compound during the reaction, resulting in the segregation of the GeSe2 binary phase and the deviation of the compound from the stoichiometric ratio, the crucible needs to be placed in the quartz tube and an additional pressure atmosphere is added. The function of the material providing the pressure gas atmosphere is to avoid excessive elemental atmosphere being deposited in the material during the cooling process, resulting in the selenium-enriched phenomenon of the synthesized BGGSe polycrystalline material, which is conducive to obtaining a near-stoichiometric ratio BGGSe polycrystalline material; and the inert gas filled in the quartz tube is to inhibit the thermal decomposition of the BGGSe compound at high temperature, resulting in the segregation of the compound composition;

[0009] 3. Step-by-step reaction: placing the sealed quartz tube into an inclined single-temperature zone tubular furnace with an inclination angle of 0.1° to 30°, heating the tubular furnace from room temperature to 683 to 685° C. at a rate of 8.0 to 10.0° C. / h, then heating to 727 to 730° C. at a rate of 12.0 to 15.0° C. / h and keeping warm for 18 to 20 hours, then heating to 1040 to 1050° C. at a rate of 15 to 18.0° C. / h and keeping warm for 90 to 100 hours; then performing 1 to 10 temperature oscillations within a temperature range of 500 to 1200° C., with a heating and cooling rate of 0.1 to 10° C. / h for each temperature oscillation, and after the temperature oscillations, cooling the tubular furnace to room temperature at a rate of 10 to 100° C. / h to obtain a high-purity polycrystalline material of selenium, germanium, gallium, and barium, which is a BaGa2GeSe6 compound with a relatively high degree of crystallinity.

[0010] Furthermore, the Ba source in step 1 is a bulk metal element barium, a powdered metal element barium, a beaded metal element barium, or a barium selenide compound (BaSe);

[0011] Furthermore, the Ga source in step 1 is bulk metal single substance gallium, liquid metal single substance gallium, bead metal single substance gallium or gallium triselenide (Ga2Se3);

[0012] Furthermore, the Ge source in step 1 is bulk single crystal germanium, powdered metallic germanium, beaded metallic germanium or germanium diselenide (GeSe2);

[0013] Furthermore, the inert atmosphere described in step 1 refers to N2, Ar or He atmosphere.

[0014] Furthermore, the built-in cylindrical crucible described in step 2 is a carbon-coated quartz crucible, a high-purity corundum crucible, a high-purity graphite crucible or a high-purity pyrolytic boron nitride crucible.

[0015] Furthermore, the vacuum state described in step 2 is to evacuate to 1×10 -4 Below Pa.

[0016] The selenium-germanium-gallium-barium compound obtained by the method of the present invention has unit cell structure parameters consistent with relevant theoretical values ​​and is a high-purity BaGa2GeSe6 compound polycrystalline material. The Ba, Ga, Ge and Se elements in the compound all conform to the stoichiometric ratio.

[0017] The BaGa2GeSe6 compound polycrystalline material of the present invention is used to grow single crystals in a vertical Bridgman single crystal growth furnace at a gradient of 5-30°C / cm, with a growth rate of 0.01-10mm / h. The grown crystal has a high transmittance of 60% in the transmittance range, and the crystal quality is good. The method of the present invention uses a "one-step method" single temperature zone to synthesize BGGSe polycrystalline material, which reduces the possibility of material exchange between the raw materials and the external environment during the synthesis process, is conducive to the synthesis of high-purity BGGSe polycrystalline material, solves the problem that the compound ratio in the "two-step method" synthesis of BGGSe is difficult to control, large-scale polycrystalline material synthesis is difficult, and polycrystalline material is susceptible to contamination, and also solves the problem that the sealed quartz tube for double-temperature zone synthesis is large in volume, is not conducive to inhibiting the decomposition of BGGSe compounds under high temperature conditions, and is difficult to obtain a uniform pure phase. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 1 is a schematic diagram of the structure of the inclined single-temperature zone tubular furnace in step 2 of Example 1; wherein 1 is a cylindrical crucible, 2 is a quartz tube, 3 is a melt in the cylindrical crucible, 4 is a substance providing a pressure gas atmosphere, and 5 is an inclined single-temperature zone tubular furnace;

[0019] Figure 2 is a photograph of the BGGSe polycrystalline material synthesized in Example 1;

[0020] Figure 3 is the XRD refinement diagram of the BGGSe polycrystalline material synthesized in Example 1;

[0021] Figure 4 This is the EDS energy spectrum of the BGGSe polycrystalline material synthesized in Example 2. DETAILED DESCRIPTION

[0022] The beneficial effects of the present invention are verified by the following examples.

[0023] Example 1: (See attached Figure 1 ) The method of preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step by using an inclined single temperature zone synthesis furnace in this embodiment is carried out according to the following steps:

[0024] 1. In a glove box with an Ar gas atmosphere, 14.010 g of bulk metal element barium (Ba), 14.011 g of bulk metal element gallium (Ga), 7.201 g of bulk metal element germanium (Ge) and 47.505 g of powdered element selenium (Se) were weighed according to the stoichiometric ratio of BaGa2GeSe6; 0.140 g of excess metal element barium (Ba) and 0.072 g of excess metal element germanium (Ge) were weighed out; 1.960 g of powdered element selenium and 5 g of GeSe2 were weighed out as substances providing a pressurized gas atmosphere;

[0025] 2. Divide the weighed materials into two groups, one group is placed in a cylindrical crucible 1, and the other group is placed in a quartz tube 2 and outside the cylindrical crucible 1; the material placed in the cylindrical crucible 1 is 14.010 g + 0.140 g of bulk metal element barium (Ba), 14.011 g of bulk metal element gallium, and 7.201 g + 0.072 g of bulk metal element germanium weighed according to a stoichiometric ratio; the material placed in the quartz tube 2 and outside the cylindrical crucible 1 is 47.505 g + 1.960 g of powdered element selenium and 5 g of GeSe2;

[0026] Then, the cylindrical crucible 1 is placed in the quartz tube 2, and the quartz tube is evacuated to a vacuum state by a molecular pump, and then an inert gas is filled into the quartz tube until the reading of the external pressure vacuum gauge reaches -0.010MPa, and the quartz tube is melted and sealed by a hydrogen-oxygen flame; in order to avoid the decomposition of the selenium-germanium-gallium-barium compound during the reaction, which leads to the segregation of the GeSe2 binary phase and the deviation of the compound from the stoichiometric ratio, the crucible needs to be placed in the quartz tube and an additional pressure atmosphere is added. The function of the material providing the pressure gas atmosphere is to avoid excessive elemental atmosphere being deposited in the material during the cooling process, which leads to selenium enrichment of the synthesized BGGSe polycrystalline material, which is conducive to obtaining a near-stoichiometric ratio BGGSe polycrystalline material; and the inert gas filled in the quartz tube is to suppress the thermal decomposition of the BGGSe compound at high temperature, which leads to the segregation of the compound components;

[0027] 2. Step-by-step reaction: the sealed quartz tube 2 is placed in an inclined single-temperature zone tubular furnace 5, the inclined angle of the inclined single-temperature zone tubular furnace 5 is 10°, the tubular furnace is slowly heated from room temperature to 683°C at a rate of 10.0°C / h, then heated to 727°C at a rate of 15.0°C / h and kept warm for 20 hours, then heated to 1050°C at a rate of 15.0°C / h and kept warm for 100 hours; then the temperature is oscillated three times in the temperature range of 800-1000°C, the heating and cooling rate of each temperature oscillation is 5°C / h, after the temperature oscillation, the tubular furnace is cooled to room temperature at a rate of 5°C / h to obtain a high-purity selenium, germanium, gallium, and barium polycrystalline material, which is a BaGa2GeSe6 compound with a relatively high degree of crystallinity.

[0028] In step 2 of this embodiment, a mixed atmosphere of Se, GeSe2 and Ar gas is used to provide a pressurized gas atmosphere. The reactions occurring during the synthesis of barium germanium gallium selenide (BGGSe) polycrystalline material are as follows:

[0029] BaGa2GeSe6 → BaGa4Se7 + GeSe2 ↑ (1)

[0030] GeSe2 → GeSe + Se ↑ (2)

[0031] The added GeSe2 is to inhibit the reaction (1), and the added Se is to inhibit the reaction (2). The mixed atmosphere of Se+GeSe2+Ar inhibits the decomposition reaction of BGGSe at high temperature, ensuring that the composition of the BGGSe polycrystalline material is close to the stoichiometric ratio during the synthesis process.

[0032] In step 3 of the present embodiment, when the temperature is raised in the first stage of the synthesis process, the high activity of Ba metal easily leads to an overly violent selenization process, resulting in the splashing of Ba-Se binary phase compounds during the reaction process, causing the final reaction product to seriously deviate from the stoichiometric ratio. Therefore, the heating rate from room temperature (30°C) to the boiling point of selenium (683°C) is selected to be a low rate of 10°C / h for heating, the purpose of which is to avoid the occurrence of segregation caused by the overly violent reaction of metal barium and elemental selenium. At the same time, the heat preservation operation is carried out at the melting point of metal Ba (727°C), the purpose of which is to completely selenize metal Ba under relatively mild conditions by controlling the reaction rate at a relatively low temperature. Subsequently, the temperature is raised to 1050°C and kept warm for 100 hours to melt the easily segregated Ga2Se3 compound (melting point is 1020°C), so that the reaction is more complete and the obtained product has better uniformity. Then the temperature is slowly lowered so that BGGSe obtains better crystallinity.

[0033] The photo of the BGGSe polycrystalline material synthesized in this embodiment by the "one-step method" in a single temperature zone is shown in Figure 2 As shown, from Figure 2 It can be seen that from Figure 2 It can be seen that the synthesized polycrystalline ingot has good crystallinity and is uniformly dark red overall. There are obvious dark red large grains in some areas, indicating that the overall chemical composition of the polycrystalline material is uniform and has a high degree of crystallinity.

[0034] The BGGSe polycrystalline powder synthesized in this example was subjected to XRD test, and the measured XRD results were subjected to Rietveld refinement using GSAS software. The refined results are shown in FIG. Figure 3 As shown in Table 1. Figure 3 It can be seen that the synthesized BGGSe polycrystalline material has a good correspondence with the X-ray diffraction peak of the standard model, and the error is small. The structure and data of the BGGSe polycrystalline material synthesized in this embodiment after Rietveld refinement are shown in Table 1. As can be seen from Table 1, the unit cell structure of the BGGSe polycrystalline material synthesized in Example 1 conforms to the three-dimensional space parameters of the R3 space group of the hexagonal system, and the unit cell volume does not change significantly. At the same time, the two different Ba-Se and (Ga / Ge)-Se chemical bond lengths are consistent with the theoretical values ​​of the perfect unit cell, indicating that the BGGSe polycrystalline material synthesized in this embodiment is a nearly stoichiometric BGGSe compound.

[0035] Table 1 Structure and data of Selenium, Germanium, Gallium and Barium polycrystalline materials

[0036]

[0037] Samples were taken from different parts of the BGGSe polycrystalline material synthesized in Example 1 to test the element content. The results are shown in Table 2.

[0038] Table 2 Element contents of different parts of synthesized BGGSe polycrystalline material in Example 1

[0039]

[0040] It can be seen from Table 2 that the BGGSe polycrystalline material synthesized in Example 1 has uniform overall composition, no other obvious impurity element content, and the content of the main component elements conforms to the stoichiometric ratio.

[0041] The BGGSe polycrystalline material synthesized in this embodiment is used to grow single crystals in a vertical Bridgman single crystal growth furnace at a gradient of 20°C / cm and a growth rate of 1mm / h. After growth, a single crystal is obtained. The single crystal has a high transmittance of 60% in the transmission range of 0.56 to 17μm and the crystal quality is good.

[0042] Embodiment 2: The method of preparing high-purity selenium, germanium, gallium, and barium polycrystalline materials for single crystal growth in one step using an inclined single-temperature zone synthesis furnace in this embodiment is carried out according to the following steps:

[0043] 1. In a glove box with an Ar gas atmosphere, 22.196 g of powdered BaSe, 14.041 g of bulk metal element gallium (Ga), 9.272 g of powdered metal element germanium (Ge) and 39.542 g of powdered element selenium (Se) were weighed, i.e., BaSe:Ga:Ge:Se=0.10 mol:0.20 mol:0.12 mol:0.50 mol; this includes the amount according to the stoichiometric ratio and the amount required for excess; 2 g of powdered element selenium and 5 g of GeSe2 were weighed as substances for providing a pressurized gas atmosphere;

[0044] 2. Divide the weighed materials into two groups, one group is mixed and ground and then placed in a cylindrical crucible, and the other group is placed in a quartz tube and outside the cylindrical crucible; the materials placed in the cylindrical crucible are 22.196 grams of powdered BaSe, 14.041 grams of bulk metal element gallium (Ga), 9.272 grams of powdered metal element germanium (Ge) and 39.542 grams of powdered element selenium (Se); the materials placed in the quartz tube and outside the cylindrical crucible are 2 grams of powdered element selenium and 5 grams of GeSe2;

[0045] Then place the cylindrical crucible in a quartz tube and use a molecular pump to evacuate the quartz tube to 10 -4Pa, then fill the quartz tube with Ar gas until the reading of the external pressure vacuum gauge reaches -0.010MPa, and finally use hydrogen-oxygen flame to melt and seal the quartz tube;

[0046] 3. Step-by-step reaction: placing the sealed quartz tube into an inclined single-temperature zone tubular furnace with an inclination angle of 10°, slowly heating the tubular furnace from room temperature to 683°C at a rate of 10.0°C / h, then heating to 727°C at a rate of 15.0°C / h and keeping warm for 20 hours, then heating to 1050°C at a rate of 15.0°C / h and keeping warm for 100 hours; then performing temperature oscillations three times in the temperature range of 800-1000°C, with a heating and cooling rate of 5°C / h for each temperature oscillation. After the temperature oscillation, cooling the tubular furnace to room temperature at a rate of 5°C / h to obtain high-purity selenium, germanium, gallium, and barium polycrystalline material, which is a BaGa2GeSe6 compound with a relatively high degree of crystallinity.

[0047] The EDS spectrum of the high-purity selenium, germanium, gallium, and barium polycrystalline material prepared in Example 2 is as follows: Figure 4 The elemental composition is shown in Table 3.

[0048] Table 3 Elemental composition of high purity selenium germanium gallium barium polycrystalline material prepared in Example 2

[0049] element Line Type wt% Wt%Sigma At% Ga L Line 17.51 0.29 20.59 Ge L Line 9.06 0.35 10.23 Se L Line 57.47 0.38 59.66 Ba L Line 15.97 0.28 9.53 Total 100.00 100.00

[0050] Depend on Figure 4 It can be seen from Table 3 that the BGGSe polycrystalline material synthesized in Example 2 does not contain impurity elements, and the main element composition conforms to the stoichiometric ratio, and the BGGSe polycrystalline material has a high purity.

Claims

1. A method for preparing high-purity selenium, germanium, gallium and barium polycrystalline materials for single crystal growth in one step using an inclined single-temperature zone synthesis furnace, characterized in that: The method proceeds as follows: In an inert atmosphere glove box, weigh Ba source, Ga source, Ge source and Se source according to the stoichiometric ratio of BaGa2GeSe6; then weigh out 0.01 wt.% ~5.00 wt.% of Ba source and 0.01 wt.% ~10.00 wt.% of Ge source added in excess; then weigh out a substance providing a pressurized gas atmosphere, wherein the substance providing a pressurized gas atmosphere is 0.01 ~ 10.00 g of elemental selenium, germanium diselenide, red phosphorus or elemental iodine; the Se source is powdered elemental selenium, beaded elemental selenium, barium selenide, gallium triselenide or germanium diselenide; The weighed materials are divided into two groups, one group is placed in a cylindrical crucible, and the other group is placed in a quartz tube and outside the cylindrical crucible; the materials placed in the cylindrical crucible are Ba source, Ga source, Ge source, compound Se source and excess Ba source and Ge source weighed according to the stoichiometric ratio; the materials placed in the quartz tube and outside the cylindrical crucible are Se source in a single substance state and a material providing a pressure gas atmosphere; Then, the cylindrical crucible is placed in a quartz tube, and the quartz tube is evacuated to a vacuum state by a molecular pump. Then, an inert gas is filled into the quartz tube until the reading of an external pressure vacuum gauge reaches -0.010 MPa, and the quartz tube is melted and sealed by a hydrogen-oxygen flame; Step-by-step reaction: placing the sealed quartz tube into an inclined single-temperature zone tube furnace, the inclined angle of the inclined single-temperature zone tube furnace is 10°~30°, heating the tube furnace from room temperature to 683~685°C at a rate of 8.0~10.0°C / h, then heating to 727~730°C at a rate of 12.0~15.0°C / h and keeping it warm for 18~20 hours, then heating to 1040~1050°C at a rate of 15~18.0°C / h and keeping it warm for 90~100 hours; then performing 1~10 temperature oscillations within a temperature range of 500~1200°C, the heating and cooling rate of each temperature oscillation is 0.1~10°C / h, after the temperature oscillation, cooling the tube furnace to room temperature at a rate of 10~100°C / h to obtain high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth.

2. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline materials for single crystal growth in one step using an inclined single temperature zone synthesis furnace according to claim 1, characterized in that: The Ba source described in step 1 is bulk metal elemental barium, powdered metal elemental barium, beaded metal elemental barium or barium selenide.

3. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline materials for single crystal growth in one step using an inclined single temperature zone synthesis furnace according to claim 1 or 2, characterized in that: The Ga source described in step 1 is bulk metal single substance gallium, liquid metal single substance gallium, bead metal single substance gallium or gallium triselenide.

4. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step using an inclined single temperature zone synthesis furnace according to claim 1 or 2, characterized in that: The Ge source described in step 1 is bulk single crystal germanium, powdered metallic germanium, beaded metallic germanium or germanium diselenide.

5. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step by using an inclined single temperature zone synthesis furnace according to claim 1 or 2, characterized in that: The inert atmosphere described in step 1 refers to N2, Ar or He atmosphere.

6. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step by using an inclined single temperature zone synthesis furnace according to claim 1 or 2, characterized in that: The built-in cylindrical crucible in step 2 is a carbon-coated quartz crucible, a corundum crucible, a graphite crucible or a pyrolytic boron nitride crucible.

7. The method for preparing high-purity selenium, germanium, gallium and barium polycrystalline material for single crystal growth in one step by using an inclined single temperature zone synthesis furnace according to claim 1 or 2, characterized in that: The vacuum state described in step 2 is to evacuate to 10 -4 Below Pa.