An asymmetric polypropylene hollow fiber degassing membrane, its preparation method and application

By optimizing the pore size and pore structure of the inner surface of the asymmetric polypropylene hollow fiber degassing membrane, the problem of large water evaporation during the degassing process of ultrapure water was solved, achieving low water evaporation, high degassing efficiency and good tolerance, thereby improving the utilization rate and economic benefits of ultrapure water.

CN117883986BActive Publication Date: 2026-11-17HANGZHOU COBETTER SEMICONDUCTOR SEPARATION MEMBRANE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410003623.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-02
Publication Date
2026-11-17
Estimated Expiration
2044-01-02

AI Technical Summary

Technical Problem

Existing hollow fiber degassing membranes have a large water evaporation rate during ultrapure water degassing, which leads to a decrease in ultrapure water utilization, affects economic efficiency, and may cause the degassing membrane to become hydrophilic, reducing the degassing rate and tolerance.

Method used

By controlling the average SEM pore size of the degassing pores on the inner surface to be no less than 40 nm, and combining appropriate pore area ratio, surface energy, average thickness, XRD crystallinity and O2 permeation, an asymmetric polypropylene hollow fiber degassing membrane was prepared, and the pore structure of the membrane was optimized to reduce water evaporation.

Benefits of technology

This technology achieves low water evaporation, high degassing efficiency, good tolerance, extended membrane lifespan, and improved economic efficiency during ultrapure water degassing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117883986B_ABST
    Figure CN117883986B_ABST
Patent Text Reader

Abstract

This invention relates to an asymmetric polypropylene hollow fiber degassing membrane, its preparation method, and its applications. The membrane comprises a main body, with one side being an inner surface facing the inner cavity and the other side being an outer surface. Non-directional tortuous pathways are formed within the main body. The average thickness of the degassing membrane is 40-80 μm, and the pore area ratio on the outer surface is no greater than 5%. The inner surface has several internal degassing pores. The surface energy of the inner surface is 25-35 mN / m. The pore area ratio on the inner surface is 10-40%. The average SEM pore size of the internal degassing pores is no less than 40 nm. The XRD crystallinity of the degassing membrane is 70%-90%. The O2 permeability of the degassing membrane is 10-80 L / (min·bar·0.1m). 2 Under a pressure of 0.4 MPa, after 12 hours, the water evaporation rate of the degassing membrane is no greater than 0.1 ml / m³. 2 / min. The degassing membrane of the present invention has a low water evaporation rate, a suitable degassing rate, and a high degassing efficiency. It can remove dissolved oxygen and other gases from ultrapure water as much as possible while minimizing ultrapure water loss, making it particularly suitable for degassing applications in the ultrapure water field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of membrane materials, and in particular to an asymmetric polypropylene hollow fiber degassing membrane, its preparation method, and its application. Background Technology

[0002] Ultrapure water generally refers to water that has undergone processes such as activated carbon, ion exchange resin, and membrane filtration to remove conductive pollutants, achieving a resistivity of 18.2 MΩ·cm (25℃). It can be used in the preparation of ultrapure materials (such as semiconductor raw materials and nano-fine ceramic materials) through distillation, deionization, reverse osmosis, or other appropriate supercritical fine technologies. Ultrapure water is commonly used in semiconductor manufacturing and medical fields. In semiconductor manufacturing applications, the gas content of ultrapure water, such as oxygen and carbon dioxide, has corresponding standards. For example, in semiconductor cleaning processes, if the oxygen content of ultrapure water does not meet the standard, it may cause the formation of amorphous silicon oxide on silicon wafers, affecting component performance and even leading to component failure. Therefore, reducing the gas content in ultrapure water has become a crucial issue in its application. Currently, hollow fiber degassing membranes are widely used for degassing various liquids, and their application in ultrapure water degassing has also been considered.

[0003] Currently, various hollow fiber degassing membranes exist on the market. For example, Japanese Patent No. JP1986101206A discloses a method for manufacturing a membrane (applied by DIC Corporation), which aims to provide a hollow fiber degassing membrane that simultaneously satisfies high gas separation capacity and high permeation rate, while also possessing high mechanical strength. Another example is Chinese Patent No. CN113226525A, which discloses an asymmetric hollow fiber membrane and its preparation and use method (applied by 3M Innovations Ltd.). Compared to other types of membranes, this asymmetric hollow fiber membrane can achieve very high gas flux and high CO2 / N2 selectivity, i.e., it has very high degassing rate and high degassing efficiency.

[0004] Similarly, in Chapter 12 of the second edition of the "Membrane Technology Handbook" edited by Deng Maicun and Jin Wanqin, which covers the gas membrane separation process, the various properties of current gas separation membranes are detailed in section 12.5, "Gas Separation Membrane Structure and Performance Characterization." Each subsection elaborates on the performance of separation membranes, such as diffusion coefficient, permeation coefficient, and pressure resistance of hollow fiber membranes. Furthermore, the doctoral dissertation from Wuhan University, "Preparation of Modified Deoxygenation Membranes and Research on Their Deoxygenation Performance," specifically introduces permeate flux, removal efficiency, and separation factor—the main parameters of deoxygenation membrane performance—in section 2.3.3, "Membrane Performance Evaluation Indicators."

[0005] Based on the publicly available patent content, books, and papers, it is clear that the degassing rate, degassing efficiency, and mechanical strength of hollow fiber degassing membranes are the performance indicators that are of great concern and importance in the application of degassing membranes.

[0006] However, through continuous research, researchers have discovered that the performance considerations for degassing membranes in ultrapure water degassing extend far beyond degassing rate, efficiency, and resilience. A currently overlooked performance aspect is water evaporation. Water evaporation refers to the amount of ultrapure water lost during degassing as gas removal continues, transforming into water vapor through evaporation and condensing along with the gas through the degassing membrane. In ultrapure water applications, the preparation process is relatively complex and difficult. As the degassing process continues, the greater the water evaporation, the greater the loss of ultrapure water, which reduces the actual utilization rate of ultrapure water and significantly lowers the economic efficiency of ultrapure water degassing. In addition, during the gas removal process, water vapor may condense into liquid water and remain on the inner surface of the degassing membrane as it flows through the membrane. The presence of liquid water in the pores on the inner surface of the degassing membrane may make it difficult for gas to pass through, thus affecting the degassing rate and efficiency. More seriously, the residue of this liquid water may cause the originally hydrophobic inner surface of the degassing membrane to become hydrophilic to a certain extent. As the ultrapure water degassing process continues, the degree of hydrophilicity of the degassing membrane will gradually increase, eventually leading to hydrophilicity on the outer surface of the degassing membrane as well. This seriously affects the durability and service life of the degassing membrane. On this basis, water vapor will also diffuse more easily into the hydrophilic areas, which may further increase the water evaporation of the degassing membrane, resulting in a large loss of ultrapure water after the degassing process. This results in low economic efficiency and practical value. Therefore, there is an urgent need for a hollow fiber degassing membrane with low water evaporation that is suitable for ultrapure water degassing. Summary of the Invention

[0007] The purpose of this invention is to provide an asymmetric polypropylene hollow fiber degassing membrane, its preparation method, and its application. By controlling the average SEM pore size of the internal degassing pores on the inner surface to be no less than 40 nm, and by having a suitable pore area ratio and surface energy on the inner surface, combined with the combined effect of a suitable average thickness of the degassing membrane, XRD crystallinity, and O2 permeation, the aim is to obtain a hollow fiber degassing membrane with low water evaporation and suitable for use in ultrapure water degassing.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: An asymmetric polypropylene hollow fiber degassing membrane includes a main body, one side of which is an inner surface facing the inner cavity, and the other side of which is an outer surface. Non-directional tortuous pathways are formed within the main body. The average thickness of the degassing membrane is 40-80 μm, and the porosity on the outer surface is no greater than 5%. The inner surface has a plurality of internal degassing pores; the surface energy of the inner surface is 25-35 mN / m; The porosity on the inner surface is 10-40%; the average SEM pore size of the inner degassing pores is not less than 40 nm. The XRD crystallinity of the degassing membrane is 70%-90%; The O2 permeation rate of the degassing membrane is 10-80 L / (min·bar·0.1m). 2 ); Under a pressure of 0.4 MPa, after 12 hours, the water evaporation rate of the degassing membrane is no greater than 0.1 ml / m³. 2 / min.

[0009] As is well known, in ultrapure water degassing applications, the degassing rate, degassing efficiency, and mechanical strength of hollow fiber degassing membranes are currently the most important performance indicators. However, the water evaporation rate of hollow fiber degassing membranes in ultrapure water degassing applications is a performance indicator that has been neglected in this field. This is because in common applications of hollow fiber degassing membranes (such as degassing solutions like ink), the degassing efficiency of the membrane determines the final gas content in the solution. The purpose of solution degassing is to minimize the gas content in the solution, thus degassing efficiency has undoubtedly become a key performance indicator. Furthermore, to increase actual production efficiency and generate greater economic value, increasing the degassing rate of the membrane has also become a key performance indicator for engineers. Moreover, when a degassing membrane possesses both degassing efficiency and degassing rate, its durability and service life have become key performance indicators for various liquid degassing applications to further enhance its practical value. As for the water evaporation rate of the degassing membrane, it has not been given much attention by technicians. This may be because, in the process of degassing liquids such as ink, even if the degassing membrane has a certain water evaporation rate, the increase in water evaporation rate has little impact on the liquids such as ink. In fact, to some extent, it may even cause the concentration of the liquids such as ink to increase to a certain extent due to the increase in water evaporation rate. Therefore, it may have driven those skilled in the art not to pay enough attention to the water evaporation rate of the degassing membrane. In other words, the proposal of the technical problem of water evaporation rate in the application of degassing membranes in ultrapure water degassing is innovative.

[0010] This is because in ultrapure water degassing applications, the preparation process of ultrapure water is relatively complex and difficult. As the ultrapure water degassing process continues, the greater the water evaporation, the greater the loss of ultrapure water, which in turn reduces the actual utilization rate of ultrapure water and greatly reduces the economic efficiency of ultrapure water degassing. In addition, during the gas removal process, water vapor may condense into liquid water and remain on the inner surface of the degassing membrane as it flows through the membrane. Due to the residue of liquid water in the pores on the inner surface of the degassing membrane, gas may have difficulty passing through the inner surface of the membrane. After long-term use of the degassing membrane for ultrapure water degassing, the degassing rate and degassing efficiency of the membrane may also be affected and decrease. More seriously, the residue of this liquid water may cause the originally hydrophobic inner surface of the degassing membrane to become hydrophilic to a certain extent. As the ultrapure water degassing process continues, the degree of hydrophilicity of the degassing membrane will gradually increase, eventually leading to hydrophilicity on the outer surface of the degassing membrane as well. This severely affects the membrane's durability and service life. Furthermore, water vapor will more easily diffuse into the hydrophilic areas, potentially leading to a further increase in water evaporation from the degassing membrane. This results in a significant loss of ultrapure water after the degassing process, leading to low economic efficiency and practical value. This invention addresses the aforementioned problems with water evaporation in ultrapure water applications by proposing an improved solution for the water evaporation performance of the degassing membrane.

[0011] As another key inventive aspect of this invention, the pore size of the internal degassing pores on the inner surface of the degassing membrane is not necessarily smaller; on the contrary, it is necessary to control the pore size of the internal degassing pores on the inner surface to have a relatively large value (the pore size of the internal degassing pores on the inner surface is not less than 40 nm), which overcomes technical bias.

[0012] It is generally believed that the water evaporation rate and degassing rate of a degassing membrane are positively correlated. As water vapor is a gas, the higher the permeation rate of the gas to be removed, the higher the permeation rate of water vapor through the degassing membrane. Based on this understanding, to effectively reduce the water evaporation rate of the degassing membrane, it is necessary to reduce the degassing rate to a certain extent. In other words, to better apply the degassing membrane in the field of ultrapure water degassing and achieve a low water evaporation rate, it may be necessary to sacrifice a certain degassing rate. Typically, the pore size on the inner surface of the degassing membrane has a significant impact on the overall membrane velocity. Therefore, even though current technicians have observed the water evaporation rate, they generally make the pore size on the inner surface of the degassing membrane smaller (e.g., 10-30 nm) to reduce the water evaporation rate, believing that this will result in a lower water evaporation rate.

[0013] However, on the contrary, we found that when the pore size of the inner surface of the degassing membrane is kept small (i.e., the pore size of the inner surface is less than 40 nm), the water evaporation of the degassing membrane does not decrease, but remains relatively high. Research revealed that this is because when the pore size of the membrane pores on the inner surface of the degassing membrane is small (less than 40 nm), water vapor undergoes capillary condensation when passing through the degassing membrane. That is, in the area near the inner surface, water vapor accumulates to a certain extent and condenses to form liquid water. As the degassing process continues, the liquid water gradually fills the membrane pores in the area near the inner surface, thus forming a "liquid film layer". It is precisely because of the presence of the liquid film layer that the area near the originally hydrophobic inner surface of the degassing membrane gradually becomes hydrophilic. With the continued degassing process, the area forming the "liquid film layer" gradually increases, that is, the degree of hydrophilicity inside the degassing membrane gradually increases, making it easier for water vapor to diffuse into the hydrophilic "liquid film layer" area, ultimately resulting in a still high water evaporation of the degassing membrane.

[0014] The degassing membrane of this invention controls the average SEM pore size of the inner degassing pores on the inner surface to be no less than 40 nm (relatively large pore size), thus significantly reducing the probability of capillary condensation of water vapor diffused into the degassing membrane, thereby effectively suppressing the formation of a "liquid film layer" near the inner surface of the degassing membrane. Furthermore, this invention further controls the pore area ratio on the inner surface to be 10-40% and the surface energy of the inner surface to be within the range of 25-35 mN / m (relatively hydrophobic), effectively suppressing capillary condensation and the formation of a "liquid film layer" due to the small pore size on the inner surface of the degassing membrane. The presence of a "liquid film layer" results in a low water evaporation rate in the degassing membrane. This is likely because, with a suitable SEM average pore size (relatively large, not less than 40 nm) for the internal degassing pores, the region near the inner surface of the degassing membrane exhibits better resistance to capillary condensation of water vapor due to the larger pore size. Simultaneously, the suitable surface energy of the inner surface (the surface tension of water is 72.8 mN / m) ensures that even if water vapor diffuses into the region near the inner surface of the degassing membrane, the relatively high surface energy between the inner surface of the degassing membrane and the condensed liquid water prevents water vapor from condensing. The differences significantly increase the difficulty for liquid water to form a "liquid film layer" in the region near the inner surface of the degassing membrane. Furthermore, even if some water vapor diffuses into the region near the inner surface of the degassing membrane, the appropriate pore area ratio and the suitable pore size of the internal degassing pores on the inner surface allow the water vapor to pass through the degassing membrane effectively without condensing and remaining within the membrane. This effectively inhibits the formation of the "liquid film layer," ultimately resulting in a lower water evaporation rate in the degassing membrane. It is particularly important to note that even if those skilled in the art can observe the degassing process... When applying membranes to ultrapure water, the water evaporation rate should be a key performance indicator. To minimize this rate, current engineers can only make the pore size of the inner surface membrane very small, and the smaller the better. Once the pore size of the inner surface membrane becomes slightly larger (e.g., greater than 40 nm), the water evaporation rate of the degassing membrane should be larger. However, contrary to this, the degassing membrane of this invention exhibits a lower water evaporation rate due to the combined effect of the inner degassing pores with a larger pore size, a suitable pore area ratio, and surface energy. This overcomes the technical biases in related understandings and is truly innovative.

[0015] To further ensure a very low water evaporation rate in the degassing membrane, this invention further modulates the XRD crystallinity, oxygen permeation rate, and average membrane thickness of the degassing membrane. This is because the degassing membrane of this invention is prepared by melt stretching, and the XRD crystallinity of the membrane essentially reflects the membrane's pore size and number to a certain extent. Similarly, the oxygen permeation rate also reflects the overall pore size and structure of the membrane. The combined effect of these two factors ensures that the membrane has a suitable pore structure and degassing rate, meaning the degassing membrane of this invention has an ideal degassing membrane structure. Furthermore, the synergistic effect of a suitable thickness (40-80 μm; the thickness should not be too low, as thickness also affects water evaporation) and the membrane's tortuous pathways further ensures an extremely low water evaporation rate. Specifically, under a pressure of 0.4 MPa, the water evaporation rate of the hollow fiber degassing membrane of this invention is no greater than 0.1 ml / m³ after 12 hours. 2 / min.

[0016] As is well known, the degassing rate is generally proportional to the degassing efficiency; that is, under normal circumstances, the higher the degassing rate, the higher the degassing efficiency. In this invention, in order to ensure that the degassing membrane has an extremely low water evaporation rate, the overall degassing rate of the membrane will not be too high. Will this affect the degassing efficiency? After multiple studies, it was found that, based on the oxygen permeability of this invention (indicating that the degassing membrane has a suitable degassing rate), combined with the corresponding crystallinity and thickness (overall pore size) and the ideal pore structure on the inner surface (internal degassing pores of suitable size and a certain pore area ratio), the degassing efficiency of the membrane was unexpectedly found to be extremely high, fully meeting the requirements for ultrapure water degassing. This was completely unexpected (achieving unexpected technical results) and is highly innovative.

[0017] In this invention, the non-directional tortuous pathways refer to randomly oriented groove structures and / or discretely distributed pore structures, and each non-directional tortuous pathway is interconnected; and the fibers forming the porous membrane structure are continuous. It can be understood that "continuous" means that essentially all the fibers are interconnected as a whole and are formed integrally without the need for additional adhesives or the like to connect them. Unless torn by external force, the network of fibers cannot be separated from each other. That is, the degassing membrane of this invention is a single-layer membrane structure, rather than a composite membrane structure.

[0018] The surface energy testing method for the outer surface of the degassing membrane of the present invention is to test the degassing membrane with a dyne pen. A 5cm long ink strip is brushed onto the degassing membrane with the dyne pen, and it is observed whether more than 90% of the ink strip shrinks and forms ink droplets within 2 seconds until it stops shrinking and ink droplets appear. The surface energy of the ink tested in this way is the surface energy of the outer surface of the membrane.

[0019] The pore area ratio of the outer and inner surfaces of the degassing membrane in this invention, as well as the average pore size of the internal degassing pores (SEM value), can all be characterized by scanning electron microscopy (SEM) of the membrane structure, followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or manually. During membrane fabrication, in the direction perpendicular to the membrane thickness (planar if the membrane is a flat sheet, and perpendicular to the radius if it is a degassing membrane), the pore size and distribution are generally uniform and consistent. Therefore, the pore area ratio in a specific region of the corresponding plane can reflect the overall pore area ratio on that plane. In actual measurement, the outer surface of the membrane fibers can be characterized using an electron microscope to obtain the corresponding SEM image. Since the pore size and distribution in the external degassing zone are generally uniform, a specific area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 100μm 2 (10μm x 10μm) or, the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the pore area ratio on this area. Perform several tests and take the average value to obtain the pore area ratio of the outer and inner surfaces of the membrane. Similarly, the SEM average pore size of the internal degassing pores can also be obtained by the above method. Of course, those skilled in the art can also obtain the above parameters by other measurement methods. The above measurement methods are for reference only.

[0020] The degassing pores in this invention may have two morphologies when observed by SEM: one is a relatively regular circular pore, and the other is a pore that is similar to an ellipse. The SEM average pore diameter of the degassing pores claimed in this invention specifically refers to the diameter of the relatively regular circular pores and the length of the minor axis of the elliptical pores.

[0021] The average thickness of the degassing membrane can be obtained by characterizing the cross-section of the degassing membrane using a scanning electron microscope, selecting six measurement points evenly on the cross-sectional SEM image of the degassing membrane, measuring the radial thickness of the six measurement points along the radial direction of the degassing membrane, and then obtaining the six measurement values ​​using computer software (such as Matlab, NIS-Elements, etc.) or manually, and calculating the average value of the six measurement values ​​to obtain the average thickness of the degassing membrane.

[0022] The XRD crystallinity of the degassed membrane refers to the XRD diffraction pattern obtained by X-ray diffraction, and the sum of the diffraction peak areas representing the crystal form and the amorphous form. The XRD crystallinity value of the degassed membrane is obtained by calculating the sum of the diffraction peak areas of the crystal form and the amorphous form.

[0023] The O2 permeation rate of the degassing membrane can be measured using the following method: Under conditions of 25°C, 0.1 bar pressure, and a membrane sample area of ​​0.1 square meters, one side of the membrane sample is subjected to the test gas (oxygen / carbon dioxide); the test gas (oxygen / carbon dioxide) is supplied into the inner cavity of the degassing membrane; the volumetric flow rate of the gas permeating through the membrane wall is measured using a flow meter (KOFLOC / 4800, Japan); the test is performed three times from the inside to the outside of the membrane and three times from the outside to the inside of the membrane, and the average value is taken. This average value is the oxygen / carbon dioxide permeation rate of the membrane, and the unit of oxygen / carbon dioxide permeation rate is ml / (min·bar·0.1m²). 2 ).

[0024] The water evaporation rate of the degassing membrane can be measured by the following test method: using the degassing membrane of the present invention as raw material, assemble it into a membrane module, connect the water channel and the module for testing, so that water fills the outer surface of the membrane fibers, control the pressure at 0.4 MPa, and after 12 hours, collect the amount of condensed water on the vacuum side of the degassing membrane.

[0025] Furthermore, the SEM average pore size of the internal degassing pores is 50-300nm, and some adjacent internal degassing pores are separated by connecting fibers. The SEM average length of the connecting fibers is 80-600nm, and the ratio of the SEM average length of the connecting fibers to the SEM average width of the connecting fibers is 1.2-25:1. The length direction of the connecting fiber is consistent with the length direction of the degassing membrane, and the width direction of the connecting fiber is consistent with the circumferential direction of the degassing membrane.

[0026] This invention controls the average SEM pore size of the degassing pores within the degassing membrane to within the range of 50-300 nm, minimizing the probability of capillary condensation near the inner surface of the degassing membrane. This effectively suppresses the formation of a "liquid film layer," resulting in lower water evaporation. Simultaneously, the relatively large pore size allows for a suitable degassing rate, ultimately leading to high degassing efficiency, making it suitable for ultrapure water degassing applications. Furthermore, the controlled average SEM pore size of the degassing pores (50-300 nm), combined with a 10-40% porosity on the inner surface and an XRD crystallinity of 70%-90%, gives the inner surface of the degassing membrane good compressive strength, as well as good tensile strength and elongation at break.

[0027] If the average SEM pore size of the internal degassing pores is too small, although the degassing membrane still has a low water evaporation rate, the increase in the final degassing rate may not be significant due to the limitation of the pore size. This may also affect the degassing efficiency of the membrane, hindering its practical application value and economic benefits in ultrapure water degassing applications. Since the inner surface of the degassing membrane is the main surface bearing the gas pressure difference during degassing, it typically needs good pressure resistance and stability during degassing. If the average SEM pore size of the internal degassing pores is too large, the degassing rate will usually increase, which may also affect the water evaporation rate. Furthermore, an excessively large average pore size may degrade the pressure resistance, mechanical strength, and stability of the inner surface during degassing, hindering continuous degassing in ultrapure water applications and potentially reducing the membrane's lifespan, thus negatively impacting economic efficiency.

[0028] In this invention, the internal degassing pores of the degassing membrane are separated by connecting fibers. Since the inner surface of the degassing membrane is subjected to relatively large gas pressure during degassing, this invention further enhances the pressure resistance of the inner surface and improves the stability of the internal degassing pores during degassing by controlling the average SEM length of the connecting fibers to be 80-600 nm and the ratio of the average SEM length to the average SEM width of the connecting fibers to be within the range of 1.2-25:1. This results in a better pressure resistance and stability of the inner surface during degassing. At the same time, controlling the average SEM length and average SEM width of the connecting fibers within a suitable range can also reduce the impact of excessively large internal degassing pore diameter on the water evaporation of the degassing membrane. This is because when the connecting fiber has a suitable aspect ratio, it can provide some support and separation for the internal degassing pores, thus avoiding the situation where the gas permeation rate is too high due to the excessively large pore size of the internal degassing pores. At the same time, combined with the appropriate XRD crystallinity and O2 permeation of the degassing membrane, the degassing membrane has a suitable degassing rate and high degassing efficiency. In addition, the degassing membrane also has a low water evaporation rate.

[0029] If the ratio of the average SEM length to the average SEM width of the connecting fibers is too large, the connecting fibers may become too long and thin, failing to effectively improve the compressive strength and stability of the inner surface. In some cases, the connecting fibers may even break under gas pressure, negatively impacting the compressive strength and degassing stability of the degassing membrane's inner surface. More seriously, if the connecting fibers break, adjacent internal degassing pores may merge, resulting in excessively large pore sizes, which could also affect the water evaporation rate of the degassing membrane. Conversely, if the ratio of the average SEM length to the average SEM width of the connecting fibers is too small, it means the average SEM length of the connecting fibers is too short. In this case, the presence of the connecting fibers may actually affect the permeation rate of gases such as oxygen in the ultrapure water, preventing a significant increase in the degassing rate of the degassing membrane despite the increased pore size, thus hindering further improvement in the degassing efficiency.

[0030] Furthermore, the internal degassing pores include a plurality of elliptical exhaust pores, the SEM average major axis of the exhaust pores is 80-800nm, the ratio of the SEM average major axis of the exhaust pores to the SEM average aperture of the exhaust pores is 1.1-18:1, and the ratio of the SEM average aperture of the exhaust pores to the SEM average width of the connecting fibers is 1.3-15:1. The major axis of the exhaust port is aligned with the length of the degassing membrane.

[0031] The internal degassing pores in this invention also include several elliptical vent holes. Compared to the circular shape of the internal degassing pores, the elliptical vent holes, with the same minor axis length as the diameter of the circular pores, have a larger area than the circular vent holes. Therefore, even when the diameter of the internal degassing pores is relatively small, the elliptical vent holes can still effectively suppress capillary condensation near the inner surface of the degassing membrane. This allows the degassing membrane to better resist the formation of a "liquid film layer" of liquid water after water vapor condensation within the internal degassing pores, resulting in a lower water evaporation rate of the degassing membrane. In this invention, the average major axis of the exhaust vent is controlled within the range of 80-800 nm using SEM. Combined with the internal degassing pores of suitable diameter and the appropriate pore area ratio of the inner surface, the exhaust vents have a relatively large air permeability area. Compared with internal degassing pores that are circular, this effectively increases the gas permeation rate and gives the degassing membrane a suitable degassing rate and high degassing efficiency. At the same time, the ratio of the average major axis of the exhaust vent to the average pore diameter of the exhaust vent (where the average pore diameter of the exhaust vent is the average minor axis of the exhaust vent, and the ratio of the major axis to the minor axis of the exhaust vent) is controlled within the range of 1.1-18:1. This ensures that although the air permeability area of ​​the elliptical exhaust vents is effectively increased, the morphology of the exhaust vents is still relatively narrow and elongated. In other words, the presence of elliptical exhaust vents does not have a significant impact on the pressure resistance and stability of the inner surface during degassing. Thus, the inner surface of the degassing membrane still has good pressure resistance and degassing stability.

[0032] This invention, by controlling the ratio of the average SEM pore size of the exhaust pores to the average SEM width of the connecting fibers within a suitable range, can further enhance the mechanical strength of the inner surface of the degassing membrane and improve the stability of degassing during internal degassing. At the same time, it can also reduce the probability of capillary condensation in the area near the inner surface of the degassing membrane to a certain extent, thereby inhibiting the formation of the "liquid film layer".

[0033] If the ratio of the SEM average pore size of the internal degassing pores to the SEM average width of the connecting fibers is too small, it means that either the SEM average pore size of the internal degassing pores is too small or the SEM average width of the connecting fibers is too large. If the SEM average pore size of the internal degassing pores is too small, although the degassing membrane still has a low water evaporation rate, the final degassing rate of the degassing membrane may not increase significantly due to the small SEM average pore size, which is not conducive to further improving the degassing efficiency of the degassing membrane. This may result in low production efficiency of the degassing membrane when applied to ultrapure water degassing, which is not conducive to actual production. If the SEM average width of the connecting fibers is too large, it may lead to an increase in the space occupied by the connecting fibers in the internal degassing pores, which may cause adjacent internal degassing pores to... There are instances of "false pores," which refer to situations where excessively thick connecting fibers occupy too much space within the internal degassing pores. Consequently, when the pore size of the internal degassing pores is relatively low, the gas flow rate through the pores is relatively low, hindering further improvement in the degassing rate. In addition, due to the presence of some elliptical vent holes on the inner surface, excessively thick connecting fibers may cause the vent holes to have excessively small pore sizes near both ends of the degassing membrane along its length. This can lead to water vapor condensing more easily in these areas. When the number of elliptical vent holes is relatively high, the pore size is relatively small, and the excessively thick connecting fibers are significant, this may also have a certain impact on the water evaporation rate of the degassing membrane.

[0034] If the ratio of the SEM average pore size of the internal degassing pores to the SEM average width of the connecting fibers is too large, it means that the SEM average pore size of the internal degassing pores is too large or the SEM average width of the connecting fibers is too small. If the average SEM pore size of the internal degassing pores is too large, it may increase the degassing rate of the degassing membrane. An excessively large degassing rate may also affect the water evaporation rate of the degassing membrane. Furthermore, an excessively large average pore size may reduce the mechanical strength of the inner surface and the stability of the internal degassing pores during degassing, potentially impacting the lifespan of the degassing membrane and hindering its continuous degassing in ultrapure water applications. Conversely, if the average SEM width of the connecting fibers is too small, during continuous degassing, adjacent internal degassing pores may break and merge due to fiber breakage, thus enlarging the average SEM pore size of the internal surface degassing pores. This could lead to fiber breakage during continuous degassing, resulting in poor stability of the internal degassing pores and potentially affecting the water evaporation rate of the degassing membrane, while also significantly reducing its lifespan.

[0035] Furthermore, the internal degassing pores are stacked to form an internal degassing zone, with some adjacent internal degassing zones separated by support regions. The SEM average width of the internal degassing zone is 90-1000 nm, the SEM average length of the internal degassing zone is at least 1.5 times the SEM average width of the internal degassing zone, and the pore density of the internal degassing zone is at least greater than 15 pores / 10 μm. 2 ; The length of the inner degassing zone is consistent with the circumferential direction of the degassing membrane, and the width of the inner degassing zone is consistent with the length of the degassing membrane.

[0036] In this invention, the degassing pores on the inner surface are not uniformly distributed, but rather concentrated in certain regions of the inner surface; these regions are referred to as the internal degassing zones. That is, several internal degassing zones exist on the inner surface, in which the internal degassing pores are stacked and arranged. The pore density of the internal degassing pores in these zones is at least greater than 15 pores / 10μm. 2 (The number of internal degassing pores in the internal degassing zone will not be too small.) Simultaneously, the appropriate pore size of the internal degassing pores ensures a suitable pore area ratio within the internal degassing zone, thereby guaranteeing a more suitable degassing rate for the entire membrane and facilitating efficient degassing. The internal degassing zone is a region with a relatively high pore area ratio on the inner surface of the membrane. It needs to have a certain area (too small an area will affect degassing efficiency, while too large an area will affect the pressure resistance of the inner surface of the membrane, thus affecting the stability of the internal degassing pores). After adjustment, its average width is 90-1000 nm. At the same time, the average SEM length of the internal degassing zone is at least 1.5 times the average SEM width of the internal degassing zone. The area of ​​the internal degassing pores will not be too small, ensuring high degassing efficiency of the membrane while having minimal impact on the pressure resistance of the inner surface of the membrane. The internal degassing pores can perform efficient degassing for extended periods.

[0037] Furthermore, the average SEM width of the support region is 50-800 nm, the ratio of the average SEM length to the average SEM width of the support region is at least greater than 2, and the porosity of the support region is less than 1%. The length of the support area is consistent with the circumferential direction of the degassing membrane, and the width of the support area is consistent with the length of the degassing membrane.

[0038] The inner surface of the degassing membrane of this invention separates two adjacent inner degassing zones through a support region (the support region is a relatively dense area on the inner surface of the membrane, with a relatively low pore area ratio of less than 1%). The SEM average width of the support region reflects the spacing between two adjacent inner degassing zones to some extent. By controlling the SEM average width of the support region to be within the range of 50-800 nm and the ratio of the SEM average length of the support region to its SEM average width to be at least greater than 2, this invention ensures that the inner surface of the degassing membrane maintains good degassing stability under continuous gas pressure difference. In other words, the inner degassing pores can still achieve good degassing stability. The pore structure of the pores can still maintain relative stability and continuously remove gas, giving the inner surface good pressure resistance and degassing stability. If the average SEM width of the support area is too small, the distance between adjacent inner degassing areas may be too small, which may lead to a relative decrease in the mechanical strength of the support area during the degassing process, thus affecting the degassing stability between adjacent inner degassing areas and hindering the continuous degassing operation of the degassing membrane. If the average SEM width of the support area is too large, it means that the distance between adjacent inner degassing areas is too large, which may result in a relatively limited increase in the degassing rate brought about by the formation of inner degassing areas on the inner surface.

[0039] Furthermore, the ratio of the average SEM width of the inner degassing zone to the average SEM width of the support zone is 1.2-3:1; The ratio of the average SEM width of the internal degassing zone to the average SEM diameter of the internal degassing pores is 1.1-10:1.

[0040] The ratio of the average SEM width of the inner degassing zone to the average SEM width of the support zone represents, to some extent, the distribution ratio of the inner degassing zone and the support zone along the length of the degassing membrane. This invention controls the ratio of the average SEM width of the inner degassing zone to the average SEM width of the support zone to be within 1.2-3:1, so that the inner surface of the degassing membrane has good pressure resistance and degassing stability, while also having a suitable degassing rate and low water evaporation. If the ratio of the average SEM width of the inner degassing zone to the average SEM width of the support zone is too large, the support zone on the inner surface of the degassing membrane may occupy a small proportion along its length. Since the inner surface of the degassing membrane is the main surface bearing gas pressure, a small proportion of the support zone may result in poor pressure resistance and degassing stability, hindering continuous degassing. Conversely, if the ratio of the average SEM width of the inner degassing zone to the average SEM width of the support zone is too small, the degassing zone may occupy a small proportion along its length, limiting the increase in degassing rate and hindering further improvement in degassing efficiency. Furthermore, in this invention, the ratio of the average SEM width of the inner degassing zone to the average SEM aperture of the inner degassing pores is controlled within the range of 1.1-10:1. This indicates the presence of a suitable number of inner degassing pores, further ensuring the degassing rate and efficiency while maintaining high pressure resistance on the inner surface of the degassing membrane.

[0041] Furthermore, the degassing membrane was tested using XRD, and the I... 14.1 The absorption intensity is between 1.8 million and 2.4 million, accounting for 25% to 55% of the total crystallization absorption intensity of the degassing membrane; Where I 14.1 The absorption intensity of the diffraction peak of the degassing membrane located near the 2θ angle of 14.1° is given.

[0042] This invention tests the degassing membrane using XRD and obtains its X-ray diffraction pattern, wherein in this invention, I 14.1 This refers to characterizing the absorption intensity at a diffraction peak near 2θ angle 14.1° after peak fitting and separation analysis of the X-ray diffraction pattern of the degassing membrane. Since the area of ​​the diffraction peak near 2θ angle 14.1° accounts for the largest proportion of the total area of ​​the XRD diffraction pattern, meaning it contributes the most to the overall pattern, and the higher the crystallinity of this crystal plane in the crystal structure, the absorption intensity of the diffraction peak near 2θ angle 14.1° is chosen to characterize the crystallinity-related performance of the degassing membrane. The total crystallinity absorption intensity of the degassing membrane is characterized by the sum of the areas of the remaining crystalline diffraction peaks after removing the amorphous diffraction peaks from the XRD diffraction pattern. The degassing membrane of this invention has I... 14.1The concentration of diffraction peaks near 14.1° 2θ within the degassing membrane indicates a high degree of crystallinity and relatively stable crystalline structure. The absorption intensity of the diffraction peak near 14.1° 2θ represents 25%-55% of the total crystal absorption intensity, signifying a relatively high crystallinity in the degassing membrane. Furthermore, the degassing membrane is prepared via a melt-stretching method. Higher crystallinity translates to a greater number of pores within the membrane. The high absorption intensity of the diffraction peak near 14.1° 2θ also contributes to the stability of the pore structure, resulting in a suitable degassing rate and good degassing stability. Additionally, higher crystallinity also leads to more suitable inter-crystal spacing, potentially increasing resistance to water vapor passage and the formation of a liquid film, thus resulting in lower water evaporation.

[0043] Furthermore, the degassing membrane was tested by XRD, and the full width at half maximum (FWHM) at a 2θ angle of 14.1° was 0.2-0.6, and the grain size was not less than 150 angstroms.

[0044] The diffraction peak at a 2θ angle of approximately 14.1° contributes the most to the overall spectrum in this invention. Therefore, the performance related to this diffraction peak at a 2θ angle of approximately 14.1° is used to characterize the crystallization-related performance of the degassing film. Half-width at half-maximum (HWHM) refers to the width of each diffraction peak in an XRD diffraction pattern, usually expressed as an angle or a 2θ value. HWHM can be used to measure the variation of lattice parameters in a crystal structure. Generally, a smaller HWHM indicates a more ordered arrangement of atoms and fewer crystal defects; a larger HWHM indicates a more disordered arrangement of atoms and more crystal defects. Therefore, the HWHM in the XRD pattern can be used to assess the quality and defect level of the crystal. The diffraction peak of this invention at a 2θ angle of approximately 14.1° has a half-width of 0.2-0.6 within a suitable range, and the grain size is not less than 150 angstroms. This means that the more ordered the atomic arrangement and the fewer the crystal defects in the degassing membrane crystal of this invention, the easier it is to form pores during the stretching process, and the more stable the pore structure formed. This results in better degassing stability of the degassing membrane. At the same time, the more ordered the atomic arrangement and the fewer the crystal defects, the better the mechanical strength and heat resistance of the degassing membrane. In addition, the more ordered the atomic arrangement and the fewer the crystal defects, the greater the resistance when water vapor passes through this region, making it difficult to form a "liquid film layer" in this region, ultimately resulting in a lower water evaporation rate of the degassing membrane.

[0045] Furthermore, the average pore size variation gradient of the degassing membrane is 0.2-6 nm / μm, and the water contact angle of the outer surface is at least greater than 100°; The average pore size variation gradient of the degassing membrane is calculated as follows: (SEM average pore size of the degassing pores inside the degassing membrane - SEM average pore size of the outer surface of the degassing membrane) / average thickness of the degassing membrane.

[0046] The average pore size gradient of the degassing membrane in this invention is controlled within 0.2-6 nm / μm, resulting in a suitable gradient between the inner and outer surfaces of the membrane. This ensures relatively low water evaporation while maintaining a relatively low overall porosity (as evidenced by XRD crystallinity). Furthermore, the suitable pore size range of the internal degassing pores reduces the likelihood of capillary condensation near the inner surface, effectively inhibiting the formation of a "liquid film layer" and further reducing water evaporation. Simultaneously, the degassing membrane exhibits a suitable degassing rate and high degassing efficiency, making it well-suited for ultrapure water degassing and possessing significant economic value.

[0047] The water contact angle of the outer surface of the present invention was measured and obtained by Krüger Scientific Instruments (Shanghai) Co., Ltd. using the Williams dynamic contact angle method with a K100 surface tension meter. In the water contact angle test, it is necessary to use tools such as glass slides to flatten the degassed membrane filaments and form a thin sheet before the water contact angle of the outer surface is tested.

[0048] The size of the water contact angle depends on the properties of the material itself and the properties of its surface. The water contact angle of the outer surface of the degassing membrane of this invention is at least greater than 100°, reflecting that the outer surface of the degassing membrane of this invention has good hydrophobicity and a suitable surface roughness. Generally, the larger the water contact angle, the better the hydrophobicity of the material, which means that the outer surface of the degassing membrane of this invention has good hydrophobicity, and the degassing membrane can have good tolerance and service life when applied to ultrapure water degassing. Due to the presence of a suitable surface roughness and a relatively hydrophobic outer surface, water vapor will encounter greater resistance when it permeates into the degassing membrane, thereby effectively suppressing the water vapor permeation rate. At the same time, the degassing membrane can ensure that the gas to be degassed has a relatively suitable permeation rate, ultimately resulting in a low water evaporation rate and a suitable degassing rate and excellent degassing efficiency.

[0049] Furthermore, the outer surface is a dense surface, and the porosity of the outer surface is less than 1%. The O2 permeation rate of the degassing membrane is 10-40 L / (min·bar·0.1m). 2 ).

[0050] The outer surface of the degassing membrane, being the side in direct contact with liquids such as ultrapure water, is a dense surface. When the pore area ratio of the outer surface is less than 1%, the outer surface of the degassing membrane has a relatively low gas permeation rate. This makes it relatively difficult for water vapor to enter the degassing membrane during the ultrapure water degassing process, thus ensuring a relatively low water evaporation rate. Furthermore, combined with the inner surface of the invention having internal degassing pores of suitable diameter and a suitable pore area ratio, the degassing rate of the degassing membrane is not significantly reduced due to the density of the outer surface. Instead, the degassing rate remains within a suitable range, resulting in high degassing efficiency. This makes the membrane suitable for application in the field of ultrapure water degassing and has high economic value.

[0051] The dense surface in this invention specifically refers to the outer surface of the degassing membrane photographed at 50,000x magnification using a scanning electron microscope, where no pore structure can be observed on the outer surface or only a very small number of pores can be observed, and the pore area ratio of the outer surface is less than 1%.

[0052] Furthermore, the outer surface has several silver-like cracks, the SEM width of the cracks is no higher than 20 nm, and the SEM average length of the cracks is 10-90 nm.

[0053] The degassing membrane of this invention has silver-crack-like cracks on its outer surface, with a SEM width of no more than 20 nm and an average SEM length controlled between 10-90 nm. Compared to a dense outer surface, the presence of cracks on the outer surface of the degassing membrane, along with the appropriate limitation of crack length and width, results in a relatively higher gas permeation rate, leading to a suitable degassing rate and high degassing efficiency. Furthermore, although the outer surface has a cracked structure, the degassing membrane of this invention has good hydrophobicity, ensuring that the permeation rate of water vapor entering the interior of the degassing membrane through the cracks remains low. Therefore, while the degassing rate is improved to a certain extent, the water evaporation rate of the degassing membrane remains low. This allows the degassing membrane with such a structure to achieve a relatively higher degassing rate and efficiency while maintaining low water evaporation when applied to the field of ultrapure water degassing, thus generating higher economic value.

[0054] Furthermore, the outer surface has an external degassing region and an external dense region. The porosity of the external dense region is less than 1%, and the external degassing region has a plurality of external degassing pores. The SEM average pore size of the external degassing pores in the external degassing region is 10-90 nm, and the density of the external degassing pores is 10-80 pores / μm. 2 ; The O2 permeation rate of the degassing membrane is 35-80 L / (min·bar·0.1m). 2 ).

[0055] The degassing membrane of this invention has an outer degassing zone and an outer dense zone on its outer surface. The outer degassing pores are concentrated in the outer degassing zone, meaning they are unevenly distributed on the outer surface. Combined with a suitable SEM average pore size (10-90 nm) and a suitable pore density within the outer degassing zone, along with a suitable inner degassing pore size and a suitable pore area ratio on the inner surface of the degassing membrane, the degassing membrane exhibits extremely high degassing rate and efficiency. This is likely because the concentrated distribution of the outer degassing pores in the outer degassing zone allows for more concentrated airflow within that zone, making oxygen and other gas molecules more prone to in-molecular collisions during permeation. This reduces the resistance to oxygen and other gases permeating through the outer degassing pores and minimizes the effects of airflow scattering and diffusion, thereby increasing the permeation rate of oxygen and other gases. Simultaneously, the presence of the outer dense zone (relatively dense with almost no pores) gives the outer surface of the degassing membrane good pressure resistance and durability. In short, with its outer surface pore structure, O2 permeation rate, and inner surface pore structure, the degassing membrane exhibits extremely high degassing rate and efficiency, while also possessing good pressure resistance and decent durability.

[0056] In this invention, the outer dense region and the outer degassing region specifically refer to the regions with small pore structures and relatively dense regions that can be clearly observed on the outer surface of the degassing membrane by SEM electron microscopy. The pore area ratio of the outer dense region is less than 1%, which means that when the outer dense region is photographed at 50,000x magnification, no pore structure can be observed or only a very small number of pores can be observed.

[0057] Furthermore, the outer surface has a plurality of uniformly distributed external degassing pores, the SEM average pore diameter of which is 10-90 nm, and the density of which is 1-30 pores / 10 μm. 2 ; The O2 permeation rate of the degassing membrane is 30-60 L / (min·bar·0.1m). 2 ).

[0058] The degassing membrane of this invention has uniformly distributed external degassing pores on its outer surface. Compared to degassing membranes with unevenly distributed external degassing pores, the uniformly distributed pores with suitable pore size and density result in a relatively lower water evaporation rate. This is because the density of external degassing pores on the outer surface of the membrane is relatively low, meaning the spacing between adjacent pores is relatively high. Combined with the relatively small pore size (10-90 nm) and the relatively hydrophobic outer surface, the rate at which water vapor enters the membrane through the pores is significantly reduced. Consequently, the membrane exhibits both high degassing rate and high degassing efficiency while maintaining a low water evaporation rate, making it particularly suitable for ultrapure water degassing applications. Furthermore, the concentrated distribution of external degassing pores within the external degassing zone primarily enhances the gas permeation rate. Similarly, the water vapor permeation rate is also increased to some extent (this increase is relative to the uniformly distributed pores; ultimately, the water vapor permeation rate observed on the outer surface remains relatively low). In addition, under the influence of such external degassing pore size and density, the degassing membrane also has relatively good tolerance, ensuring the service life of the degassing membrane in ultrapure water degassing applications.

[0059] In this invention, the uniformly distributed external degassing pores specifically refer to the fact that, through multiple observations of the outer surface of the degassing membrane using SEM electron microscopy, it can be clearly observed that there are basically no relatively dense areas on the outer surface of the degassing membrane, and the membrane pores are basically uniformly distributed on the outer surface.

[0060] Furthermore, the main body includes a skin layer and a support layer. One side of the support layer is an inner surface, and one side of the skin layer is an outer surface. The other side of the skin layer and the other side of the support layer are transitioned by continuous fibers. The thickness of the skin layer is 0.1-3 μm. The support layer contains porous fibers for forming a porous structure. The average SEM diameter of the porous fibers is 10-120 nm, and the density of the porous fibers is 30-450 fibers / μm. 2 .

[0061] The thickness of the degassing membrane layer in this invention is controlled within a suitable range (0.1-3 μm), combined with a suitable diameter (10-120 nm) and quantity (30-450 per μm) in the support layer. 2The combined effect of porous fibers results in a degassing membrane with low water evaporation while maintaining a suitable degassing rate and high degassing efficiency. This is because the porosity of the membrane skin is relatively low, and combined with the overall relatively strong hydrophobicity of the membrane, the resistance to water vapor permeation within the skin is greatly increased. Therefore, the membrane can achieve low water evaporation at this skin thickness, while also exhibiting good durability, ensuring its lifespan in ultrapure water degassing applications. Furthermore, the porous fiber support layer with its specific pore size and density provides the membrane with good pressure resistance and degassing stability due to the internal pore structure. The combined effect of these porous fibers of such diameter and quantity reflects a suitable number of non-directional tortuous pathways within the support layer, resulting in a good degassing rate. Although the porosity within the support layer is relatively high, the water vapor permeation rate within it remains slow, due to the combined effect of the porous fibers (hydrophobicity) and the tortuous pathways within the membrane. It is precisely due to the combined effect of such a skin thickness and support layer structure that the degassing membrane has a low water vapor content, while also having a suitable degassing rate and high degassing efficiency, as well as good mechanical strength (tensile strength and elongation at break) and membrane pore stability during degassing, which can better meet the needs of ultrapure water degassing applications.

[0062] The degassing membrane of the present invention comprises a skin layer and a support layer. Specifically, by observing the cross-sectional structure of the degassing membrane using SEM electron microscopy, it was found that the main structure of the degassing membrane mainly includes two regions. The skin layer refers to a certain region (near the outer surface) where the membrane pore size is very small and the porosity is low. The support layer refers to a certain region (near the inner surface) where the membrane pore size is relatively large and the porosity is relatively high.

[0063] Furthermore, the minimum thickness of the degassing membrane is not less than 30 μm, and the difference between the maximum thickness and the minimum thickness of the degassing membrane is not greater than 15 μm.

[0064] The minimum thickness of the degassing membrane of this invention is not less than 30 μm, and the difference between the maximum and minimum thickness of the degassing membrane is not greater than 15 μm. This reflects that the thickness of the degassing membrane of this invention is relatively uniform, which avoids the impact of water evaporation caused by uneven thickness of the degassing membrane. This is because if the minimum thickness of the degassing membrane is too small, the area with the minimum thickness of the degassing membrane may become a "breakthrough point" for gas permeation during degassing, making the path and resistance of water vapor permeation through the degassing membrane relatively small, which may ultimately affect the water evaporation of the degassing membrane. At the same time, the difference between the maximum and minimum thickness of the degassing membrane is not greater than 10 μm, so that the degassing membrane can also have relatively good tensile strength and elongation at break.

[0065] In this invention, the maximum and minimum thicknesses refer to the maximum and minimum thicknesses of the degassing membrane obtained by repeatedly observing the cross-section of the degassing membrane using SEM electron microscopy, measuring it using computer software (such as Matlab, NIS-Elements, etc.) or manually, and then performing corresponding calculations.

[0066] Furthermore, the CO2 permeation rate of the degassing membrane is 10-90 L / (min·bar·0.1m). 2 ); The deoxygenation efficiency of the degassing membrane is greater than or equal to 90%; The tensile strength of the degassing membrane is not less than 200 CN, and the elongation at break is 50-500%.

[0067] The degassing membrane in this invention possesses good tensile strength and elongation at break. It also exhibits suitable removal rates for both oxygen and carbon dioxide, and demonstrates a high deoxygenation efficiency exceeding 90%. This effectively removes dissolved oxygen and other gases from ultrapure water. Crucially, the membrane also exhibits low water evaporation, making it suitable for degassing applications in ultrapure water. The deoxygenation efficiency is used to represent the degassing efficiency in this invention primarily because the oxygen content in ultrapure water significantly impacts subsequent processing steps (such as silicon wafer cleaning), and the oxygen content in ultrapure water is generally high.

[0068] The test method for CO2 transmission can be the same as that for O2 transmission. The deoxygenation efficiency of this invention can be achieved by assembling a membrane module using the degassing membrane of this invention as raw material, and connecting the module to the process section and polishing section of the ultrapure water preparation process. Under rated flow conditions, the inlet water temperature is tested at 25 ℃, and the inlet water oxygen concentration should meet the following requirements: the inlet water oxygen concentration of the deoxygenation membrane module in the process section is 6-8 mg / L and the inlet water oxygen concentration of the deoxygenation membrane module in the polishing section is ≤10 μg / L. The absolute vacuum degree is 0.006 MPa, and the nitrogen purging rate is 0.012 times the rated flow rate of the inlet water. The deoxygenation efficiency of the deoxygenation membrane module is tested respectively. In this invention, deoxygenation efficiency is used to represent degassing efficiency, mainly because the oxygen content in ultrapure water has a significant impact on semiconductor applications, and the oxygen content in ultrapure water is generally relatively high.

[0069] The tensile strength and elongation at break of the degassed membrane can be tested using the following method: At room temperature, the degassed membrane sample is stretched uniformly using a tensile testing machine (stretching speed 50 mm / min, upper and lower clamp distance 30 mm) until the membrane breaks. The tensile strength and elongation at break are then measured. This process is repeated three times, and the average value is taken. This average value is the final tensile strength and elongation at break value of the membrane. When testing the tensile strength and elongation at break of the degassed membrane, it is usually necessary to maintain a consistent inner diameter, for example, by keeping the inner diameter at 0.2 mm before conducting the tests.

[0070] Furthermore, the present invention also provides a process for preparing an asymmetric polypropylene hollow fiber degassing membrane, comprising the following process steps: S1. Spinning: PP material is melted and extruded through a die, and a molded product with a hollow inner cavity is formed under the action of an inert gas as the core liquid; wherein the die extrusion temperature is at least greater than 210℃. The weight-average molecular weight of PP material is 100,000-800,000, the molecular weight distribution index is 1.5-7, and the isotacticity of PP material is not less than 95%. S2. Pre-crystallization: The molded product is placed in an air section for pre-crystallization. The temperature of the air section is 30-120℃, and the pre-crystallization time is 0.05-0.6s. The inert gas flow rate is 0.5-4 ml / min, the temperature of the inert gas in the air section is 80-130℃, and the temperature of the inert gas in the air section is higher than the ambient temperature of the air section. S3, air-cooled crystallization: the molded product obtained in step S2 is cooled by blowing air to obtain nascent fibers, wherein the blowing temperature is 30-70℃ and the blowing speed is 20-100m / min; S4, one-time heat setting, involves the first heat setting treatment of the nascent fibers to obtain a heat-set semi-finished product; S5, cold drawing to form holes: the heat-set semi-finished product is cold-drawn, wherein the ratio of the cold drawing temperature to the temperature of the inert gas in the air section satisfies 1:(2.5-6), and the cold-drawn semi-finished product is obtained. S6, hot drawing to expand the hole, the cold-drawn semi-finished product is hot drawn to expand the hole, wherein the ratio of the hot drawing temperature to the cold drawing temperature satisfies (3-7):1, and the hot-drawn semi-finished product is obtained; S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process to obtain a hollow fiber degassed membrane.

[0071] Furthermore, in step S1, the melting process includes melting, mixing and metering steps. The metering temperature is 2-10°C higher than the die extrusion temperature. The die extrusion temperature is preferably 215-230°C, and the length-to-diameter ratio of the die is 2-6.

[0072] Furthermore, in step S4, the heat-set semi-finished product is slightly stretched with an elongation of 0.5-3%, the temperature of the first heat setting is 120-150℃, and the time of the first heat setting is 60-150 min. In step S7, the second heat setting temperature is 10-30°C higher than the first heat setting temperature, and the second heat setting time is 0.5-3 minutes.

[0073] Furthermore, in step S5, the cold drawing elongation rate is 20%-40%, and the cold drawing rate is 10-30% / min; In step S6, the hot stretching elongation is 80%-120%, and the hot stretching rate is 0.3-1.3% / min.

[0074] This invention prepares an asymmetric polypropylene hollow fiber degassing membrane using a melt stretching method. Compared to the thermally induced phase separation method, the asymmetric polypropylene hollow fiber degassing membrane of this invention does not require the addition of additional solvents, non-solvents, or other additives during the preparation process. Its raw material is only polypropylene, which enables the polypropylene hollow fiber degassing membrane to have high purity when applied to the ultrapure water field. It minimizes the risk of contamination of the ultrapure water purity due to the leaching of additives in the degassing membrane, making it particularly suitable for ultrapure water applications.

[0075] It is expected that the relevant properties of the raw materials are fundamental to determining the surface properties and microporous structure of the membrane fibers. Research has shown that parameters such as the weight-average molecular weight, molecular weight distribution index, and isotacticity of polypropylene (PP) materials have a significant impact on film formation performance. Isotacticity refers to the distribution of methyl groups on the polypropylene molecular chain. The isotacticity of the polypropylene raw material in this invention is not less than 95%, meaning that the more regularly the methyl groups on the molecular chain are arranged, the more complete the crystal structure is formed during melt stretching, and the easier it is to obtain an ideal membrane structure. If the isotacticity of the polypropylene material is low, it may result in fewer pore structures in the film, or although a relatively suitable number of pore structures can be formed, the stability of the pore structure and various performance parameters of the film formation cannot meet the requirements, which may seriously affect the degassing rate, degassing efficiency, and water evaporation of the degassed membrane. By controlling the molecular weight distribution index of the polypropylene material within the range of 1.5-7, combined with the weight-average molecular weight of the polypropylene material within the range of 100,000-800,000, we found that the polypropylene material has good processing fluidity after melting, and at the same time, under the action of stretching attraction, it is endowed with a certain orientation, which is beneficial for preparing an ideal membrane structure.

[0076] In step S1 of this invention, the polypropylene (PP) material is first melted (mainly through raw material conveying, extrusion, and preheating, gradually melting the material until it reaches a fully molten state), mixed (mainly through raw material mixing, compression, and pressurization for degassing), and metered (mainly through mixing, melting, and conveying, providing sufficient pressure to maintain uniform raw material temperature and stable melt flow). This invention controls the metering temperature to be 2-10°C higher than the die extrusion temperature. When the molten polypropylene material is extruded through the die, internal heat conduction occurs, lowering its temperature. During this cooling process, the temperature of the inner and outer surfaces becomes more uniform, ensuring a relatively sufficient crystallization process. This, in turn, ensures a relatively stable pore structure in the prepared membrane, which is more conducive to forming a suitable membrane pore structure. Furthermore, by controlling the die aspect ratio to 2-6, the macromolecular chains of the molten polypropylene material undergo shear force during flow, resulting in orientation and easier formation of crystal nuclei. This gives the final membrane filaments a suitable degree of crystallinity, resulting in a more stable pore structure and greater tensile strength and elongation at break in the prepared membrane. Meanwhile, inert gas is used as the core liquid during the melt extrusion process, which enables the degassed film to have a relatively uniform thickness after molding.

[0077] As one of the important conditions of the process steps of this invention, the extrusion temperature of the die head is controlled to be at least greater than 210°C, and more preferably 215-230°C. The further increase in the extrusion temperature of the die head results in a higher initial temperature for the molten polypropylene, which to some extent increases the time for the polypropylene material to crystallize (when other factors are the same, such as the cooling rate, the crystallization temperature of polypropylene is consistent, that is, the time for the crystallization process is increased by the higher initial temperature). This is beneficial for the area near the inner surface of the molded product to have a longer time to crystallize and form an internal degassing pore structure with a relatively large pore size.

[0078] Based on this, the molded product is extruded through the die and then enters the air section for pre-crystallization. This invention controls the appropriate air section temperature (30-120℃) and residence time (i.e., the pre-crystallization time is 0.05-0.6s) to enable the molded product to undergo a suitable pre-crystallization process and generate a suitable number and size of crystal nuclei, so as to prepare an ideal membrane structure. The temperature of the air section and the pre-crystallization time mainly affect the structure acting on the outer surface of the degassed membrane (when the temperature of the air section is relatively high and the pre-crystallization time is relatively long, the outer surface of the degassed membrane also has relatively sufficient time to form a suitable size and number of crystal nuclei, and after stretching and pore formation, a certain pore structure is formed on the outer surface; as the temperature of the air section and the pre-crystallization time decrease, the number of crystal nuclei generated on the outer surface of the degassed membrane gradually decreases, and even fails to form crystal nuclei of a suitable size, resulting in a membrane pore structure with crack structure or dense outer surface after stretching and pore formation).

[0079] As another important condition in the process steps of this invention, in step S2, the temperature of the inert gas used as the core liquid in the air section is 80-130℃ and the temperature of the inert gas in the air section is higher than the ambient temperature of the air section. The flow rate of the inert gas is controlled within the range of 0.5-4ml / min. That is, by reasonably controlling the temperature and flow rate of the core liquid (inert gas) in the air section, this invention further reduces the cooling rate of the area near the inner surface of the molded product, so that the inner surface of the molded product has sufficient time to form a suitable number and size of crystal nuclei. Finally, after stretching and forming holes, a relatively large internal degassing pore structure is formed, which ensures that the degassing membrane of this invention has a low water evaporation rate and a suitable degassing rate. Furthermore, it can be understood that the ambient temperature of the air section primarily affects the outer surface. Under normal circumstances, the inner surface cools at a lower rate than the outer surface, while the temperature of the core liquid (inert gas) primarily affects the inner surface. Based on this, this invention controls the temperature of the inert gas (core liquid) within the air section to be higher than the ambient temperature of the air section, resulting in a slower cooling rate of the inner surface. This explains the significant difference in pore size between the inner and outer surfaces of the membrane fiber, with the inner surface having a relatively larger pore size. Consequently, the final membrane fiber exhibits lower water evaporation, a suitable degassing rate, and higher degassing efficiency, effectively meeting the requirements of ultrapure water applications. The inert gas used as the core liquid can be any one of nitrogen, argon, or helium.

[0080] Then, the pre-crystallized molded product is cooled and crystallized by blowing air. After the pre-crystallization process in the air section, a certain number and size of crystal nuclei are formed inside the molded product. This invention controls the appropriate blowing temperature (30-70℃) and blowing speed (20-100m / min) to form a suitable number and size of crystal nuclei in the molded product, thereby preparing the membrane filaments with an ideal membrane structure (for example, when the blowing temperature is low and the blowing speed is high, combined with the high temperature and pre-crystallization time in the air section, that is, "heat preservation" (referring to the relatively high temperature in the air section) and relatively sufficient time for pre-crystallization are carried out in the air section, and "extreme cooling" (referring to the rapid cooling rate in the air-cooled crystallization section) is used to quickly cool down the product. Under the combined effect of the air section and the air-cooled crystallization section, the outer surface is formed with an unevenly distributed membrane pore structure, while the inner surface has a relatively large membrane pore structure).

[0081] Next, the nascent fibers undergo a first heat setting. Preferably, the first heat setting process involves slight stretching with an elongation of 0.5-3%, and the temperature is controlled at 120-150°C for 60-150 minutes. Polypropylene typically crystallizes at around 120°C (the crystallinity of polypropylene fluctuates due to factors such as molecular weight). By controlling the temperature of the first heat setting, this invention allows the nascent fibers to recrystallize to some extent during the first heat setting process. This enables recrystallization within the nascent fibers, building upon the air-cooled crystallization stage, and the generation of a suitable number and size of crystal nuclei. Also taking into account the recrystallization process of the nascent fibers, the first heat setting temperature of this invention is controlled within the range of 60-150 min, so that the nascent fibers have a relatively suitable time for recrystallization, ultimately enabling the inner surface of the degassed membrane to form a membrane pore structure with a relatively large pore size. In addition, we found that slightly stretching the nascent fibers during the first heat setting process also helps to form a membrane pore structure with a large inner surface pore size, uniform distribution, and a suitable pore area ratio.

[0082] After the first heat setting, the heat-set semi-finished product undergoes a cold drawing process. The main purpose of the cold drawing process is to open up the crystal nuclei inside the heat-set semi-finished product and form a porous structure. This is also one of the important steps in this invention to achieve a relatively large internal degassing pore structure on the inner surface of the membrane fiber. This invention controls the ratio of the cold drawing temperature to the inert gas temperature in the air section to be within the range of 1:(2.5-6). Preferably, the cold drawing elongation is controlled within 20%-40%, and with a cold drawing rate of 10-30% / min, a relatively uniform membrane pore structure with large pores is formed on the inner surface of the degassing membrane. This is likely because the core liquid (inert gas) continuously affects the inner surface of the molded product during the air section process, which to some extent determines the number, size, and distribution of crystal nuclei on the inner surface. If the ratio of the cold drawing temperature to the temperature of the core liquid (inert gas) in the air section is too small, it may result in the lamellar structure not being able to be pulled apart well to form a suitable pore structure during the stretching process, which may result in the membrane pore diameter of the internal degassing pores being relatively small. If the ratio of the cold drawing temperature to the temperature of the core liquid (inert gas) in the air section is too large, it may result in the crystal nuclei near the inner surface being overstretched during the stretching process, which may result in the inability to form a suitable membrane pore structure.

[0083] After cold drawing to create pores, the cold-drawn semi-finished product is then subjected to hot drawing to expand the pores. In this invention, the ratio of the hot drawing temperature to the cold drawing temperature is controlled to satisfy (3-7):1. Preferably, the hot drawing elongation is controlled at 80%-120%, and the hot drawing rate is controlled at 0.3-1.3% / min. This is because certain residual stress will appear in the cold-drawn semi-finished product during the cold drawing process. Different cold drawing rates result in different pore structures, and the internal residual stress will also be different. This invention, through the coordination between the hot drawing temperature and the cold drawing temperature (i.e., the ratio of the hot drawing temperature to the cold drawing temperature satisfies (3-7):1), enables the final acquisition of an ideal membrane pore structure. If the ratio of the hot drawing temperature to the cold drawing temperature is too small, the micropore structure formed in the cold drawing stage may not be able to stretch and enlarge well, thus failing to obtain an internal degassing pore structure with a relatively large inner surface pore size. If the ratio of the hot drawing temperature to the cold drawing temperature is too large, the micropores generated in the cold drawing stage may be excessively enlarged due to the hot drawing process, resulting in a relatively large pore size of the degassing membrane, which may affect the pressure resistance and degassing stability of the degassing membrane.

[0084] Finally, the cold-drawn semi-finished product undergoes a second heat-setting treatment. Preferably, the second heat-setting temperature is 10-30℃ higher than the first, and the second heat-setting time is 0.5-3 minutes. Research shows that controlling the second heat-setting temperature within the range of 10-30℃ higher than the first temperature significantly avoids the melting of the boundaries between adjacent pore structures due to excessively high heat-setting temperatures after cold drawing, which could lead to the fusion of adjacent pore structures. This minimizes the impact on the mechanical strength and degassing rate of the degassed membrane after the second heat-setting, resulting in a final membrane with good mechanical strength and a good degassing rate. Furthermore, the second heat-setting effectively eliminates residual stress from the stretching and pore-forming stage without damaging the membrane pore structure, thus ensuring that the inner surface of the degassed membrane has a pore structure with a suitable pore size, resulting in a final degassed membrane with low water evaporation.

[0085] Furthermore, the present invention also provides an application of an asymmetric polypropylene hollow fiber degassing membrane, which is used in applications such as ultrapure water degassing.

[0086] In summary, the present invention has at least one of the following beneficial technical effects: 1. The asymmetric polypropylene hollow fiber degassing membrane of the present invention, through the combination of internal degassing pores with appropriate pore size (relatively large pore size), appropriate internal surface pore area ratio and surface energy of the internal surface, combined with the appropriate thickness of the degassing membrane, XRD crystallinity and O2 permeation, enables the degassing membrane of the present invention to reduce the probability of capillary condensation within the degassing membrane and effectively suppress the formation of a "liquid film layer". This results in a lower water evaporation rate for the degassing membrane of the present invention. At the same time, the degassing membrane of the present invention also has a suitable degassing rate and high degassing efficiency, making it particularly suitable for application in the field of ultrapure water degassing.

[0087] 2. The present invention achieves a degassing membrane with low water evaporation while maintaining extremely high degassing rate and efficiency by combining external degassing pores with suitable pore size and uneven distribution on the outer surface and internal degassing pores with suitable pore size and concentrated distribution in the internal degassing zone. This allows the degassing membrane to minimize the gas content in ultrapure water. Attached Figure Description

[0088] The present invention will be further described below with reference to the accompanying drawings: Figure 1 The image shown is a scanning electron microscope image of the inner surface of the hollow fiber degassing membrane prepared in Example 1, with a magnification of 50K×. Figure 2 The image shown is a scanning electron microscope image of the inner surface of the hollow fiber degassing membrane prepared in Example 1, with a magnification of 10K×. Figure 3 The image shown is a scanning electron microscope image of the outer surface of the hollow fiber degassing membrane prepared in Example 2, with a magnification of 1K×. Figure 4 The image shown is a scanning electron microscope image of the outer surface of the hollow fiber degassing membrane prepared in Example 2, with a magnification of 10K×. Figure 5 The image shown is a scanning electron microscope image of the outer surface of the hollow fiber degassing membrane prepared in Example 5, with a magnification of 20K×. Figure 6 The image shown is a scanning electron microscope (SEM) image of the cross-section of the hollow fiber degassing membrane prepared in Example 1, with a magnification of 100K×. Detailed Implementation

[0089] The present invention will be further described in detail below with reference to the embodiments. Unless otherwise specified, the raw materials and equipment used to prepare the filter membrane in the following embodiments can be purchased commercially. Example 1

[0090] A method for preparing an asymmetric polypropylene hollow fiber degassing membrane includes the following process steps: S1, spinning, where PP material is melted and extruded through a die, forming a molded product with a hollow inner cavity under the action of an inert gas as the core liquid; wherein the die extrusion temperature is at least greater than 210°C; wherein the inert gas as the core liquid is nitrogen. In step S1, the melting process includes melting, mixing and metering steps. The metering temperature is 5°C higher than the die extrusion temperature. The metering temperature is 235°C, the die extrusion temperature is 230°C, and the die length-to-diameter ratio is 6. The weight-average molecular weight of the PP material is 800,000, the molecular weight distribution index is 1.5, and the isotacticity of the PP material is not less than 95%. S2, Pre-crystallization: The molded product is placed in an air section for pre-crystallization. The temperature of the air section is 120℃, and the pre-crystallization time is 0.6s. The inert gas flow rate is 0.8 ml / min, the temperature of the inert gas in the air section is 125℃, and the temperature of the inert gas in the air section is higher than the ambient temperature of the air section. S3, air-cooled crystallization, the molded product obtained in step S2 is cooled by blowing air to obtain nascent fibers, wherein the blowing temperature is 35℃ and the blowing speed is 100m / min; S4, First heat setting: The nascent fibers undergo a first heat setting treatment, with slight stretching of the nascent fibers to an elongation of 2.8%. The temperature for the first heat setting is 150℃, and the time for the first heat setting is 60 minutes, resulting in a heat-set semi-finished product. S5, cold drawing to form holes, the heat-set semi-finished product is cold drawn, the cold drawing temperature is 30℃, the cold drawing elongation rate is 40%, and the cold drawing rate is 10% / min, to obtain the cold drawn semi-finished product. S6, hot drawing and hole expansion: The cold-drawn semi-finished product is hot-drawn and hole-expanded, wherein the hot drawing temperature is 140℃, the hot drawing elongation is 120%, and the hot drawing rate is 1.3% / min, to obtain the hot-drawn semi-finished product; S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process. The second heat setting temperature is 10°C higher than the first heat setting temperature. The second heat setting temperature is 160°C, and the second heat setting time is 0.5 min, resulting in a hollow fiber degassed membrane.

[0091] Examples 2-8

[0092] The difference between Examples 2-8 and Example 1 lies in the different process parameters, as shown in Tables 1-1 and 1-2. In Examples 2 and 8, the inert gas used as the core fluid is nitrogen; in Examples 3-4, the inert gas used as the core fluid is helium; and in Examples 5-7, the inert gas used as the core fluid is argon. Comparative Example 1

[0093] The difference between Comparative Example 1 and Example 6 lies in the different process parameters, as shown in Tables 1-1 and 1-2. (After morphological characterization, it was found that the outer surface of the degassing membrane in Comparative Example 1 was relatively dense with almost no pore structure, and the pore size on the inner surface of the degassing membrane was relatively small with a low pore area ratio, making it impossible to form an internal degassing zone.) Comparative Example 2

[0094] The difference between Comparative Example 2 and Example 6 lies in the different process parameters, as shown in Tables 1-1 and 1-2. (After morphological characterization, it was found that the outer surface of the degassing membrane in Comparative Example 2 was relatively dense with almost no pore structure, and the pore size on the inner surface of the degassing membrane was relatively small with a low pore area ratio, making it impossible to form an internal degassing zone.) Table 1-1

[0095] Table 1-2

[0096] Membrane structure parameter detection The morphology of the PP hollow fiber degassing membranes prepared in Examples 1-8 and Comparative Examples 1-2 was characterized using a scanning electron microscope (Hitachi S-5500). The outer surface, inner surface, and cross-section of the PP hollow fiber degassing membrane were selected as the observation objects. The specific detection and measurement results are shown in Tables 2-1 and 2-2.

[0097] Table 2-1

[0098] Table 2-2

[0099] The thickness of the skin layer of the hollow fiber degassing membranes prepared in Examples 5-7 and Comparative Examples 1-2 was measured, and the pore size and density of the porous fibers in the cross section of the hollow fiber degassing membranes prepared in Examples 1-2 and Example 8 were measured. The test results are shown in Tables 2-3 and 2-4.

[0100] Table 2-3

[0101] Table 2-4

[0102] Membrane performance parameter testing 1.1 Tensile strength and elongation at break tests After testing, the tensile strength of the PP hollow fiber degassing membranes prepared in Examples 1-8 is not less than 200 CN, and the elongation at break is 50-500%, which means that they all have large tensile strength and elongation at break, and can meet the needs of industrialization.

[0103] 1.2 Surface energy test; 1.3 Water evaporation test; 1.4 Oxygen and carbon dioxide permeability test; 1.5 Deoxidation efficiency test; 1.6 XRD crystallinity test.

[0104] The test results are shown in Table 3.

[0105] Table 3

[0106] As can be seen from the above, the hollow fiber degassing membranes prepared in Examples 1-8 of the present invention all have low water evaporation, which minimizes the loss of ultrapure water caused by gas removal when applied in the field of ultrapure water degassing, thus improving the utilization rate of ultrapure water. Furthermore, the hollow fiber degassing membranes prepared in Examples 1-8 of the present invention also have excellent degassing efficiency, all exceeding 90%. In addition, the degassing membranes also have high O2 and CO2 permeability, i.e., good degassing rate. When applied to ultrapure water degassing, they can almost completely remove the gas from the ultrapure water, and have a relatively fast degassing rate, resulting in high production efficiency and high economic value in degassing applications. Even after a long-term endurance test (one year of use), the hollow fiber degassing membranes prepared in Examples 1-8 of the present invention can still maintain a high degassing rate and degassing efficiency while still having low water evaporation. The degassing membranes prepared in Comparative Examples 1 and 2 had high water evaporation rates and low degassing rates and efficiencies, which could not meet the requirements of ultrapure water applications.

[0107] The preferred embodiments of the present invention have been described in detail above. However, it should be understood that after reading the above teachings, those skilled in the art can make various alterations or modifications to the present invention. These equivalent forms also fall within the scope defined by the appended claims.

Claims

1. An asymmetric polypropylene hollow fiber degassing membrane, comprising a main body, one side of which is an inner surface facing the inner cavity, and the other side of which is an outer surface, wherein a non-directional tortuous pathway is formed within the main body, characterized in that: The average thickness of the degassing membrane is 40-80 μm, and the porosity on the outer surface is no greater than 5%. The inner surface has a plurality of internal degassing pores; The surface energy of the inner surface is 25-35 mN / m; The porosity on the inner surface is 10-40%; the average SEM pore size of the inner degassing pores is 50-300 nm. The XRD crystallinity of the degassing membrane is 70%-90%; The O2 permeation rate of the degassing membrane is 10-80 L / (min·bar·0.1m). 2 ); Under a pressure of 0.4 MPa, after 12 hours, the water evaporation rate of the degassing membrane is no greater than 0.1 ml / m³. 2 / min.

2. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: Some adjacent internal degassing pores are separated by connecting fibers, the average SEM length of the connecting fibers is 80-600nm, and the ratio of the average SEM length of the connecting fibers to the average SEM width of the connecting fibers is 1.2-25:

1. The length direction of the connecting fiber is consistent with the length direction of the degassing membrane, and the width direction of the connecting fiber is consistent with the circumferential direction of the degassing membrane.

3. The asymmetric polypropylene hollow fiber degassing membrane according to claim 2, characterized in that: The internal degassing pores include several elliptical venting pores. The average major axis of the venting pores in SEM is 80-800 nm. The ratio of the average major axis of the venting pores in SEM to the average pore diameter in SEM is 1.1-18:

1. The ratio of the average pore diameter in SEM to the average width of the connecting fiber in SEM is 1.3-15:

1. The major axis of the exhaust port is aligned with the length of the degassing membrane.

4. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The internal degassing pores are stacked to form an internal degassing region. Some adjacent internal degassing regions are separated by support regions. The SEM average width of the internal degassing region is 90-1000 nm, the SEM average length of the internal degassing region is at least 1.5 times the SEM average width of the internal degassing region, and the pore density of the internal degassing region is at least greater than 15 pores / 10 μm. 2 ; The length of the inner degassing zone is consistent with the circumferential direction of the degassing membrane, and the width of the inner degassing zone is consistent with the length of the degassing membrane.

5. The asymmetric polypropylene hollow fiber degassing membrane according to claim 4, characterized in that: The average SEM width of the support region is 50-800 nm, the ratio of the average SEM length to the average SEM width of the support region is at least greater than 2, and the porosity of the support region is less than 1%. The length of the support area is consistent with the circumferential direction of the degassing membrane, and the width of the support area is consistent with the length of the degassing membrane.

6. The asymmetric polypropylene hollow fiber degassing membrane according to claim 4, characterized in that: The ratio of the average SEM width of the internal degassing zone to the average SEM width of the support zone is 1.2-3:1; The ratio of the average SEM width of the internal degassing zone to the average SEM diameter of the internal degassing pores is 1.1-10:

1.

7. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The degassing membrane was tested using XRD. 14.1 The number is between 1.8 million and 2.4 million, of which I 14.1 The absorption intensity is the diffraction peak of the degassing membrane located near the 2θ angle of 14.1°, which accounts for 25%-55% of the total crystal absorption intensity of the degassing membrane.

8. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The degassing membrane was tested by XRD and found to have a full width at half maximum (FWHM) of 0.2-0.6 near a 2θ angle of 14.1°, with a grain size of not less than 150 angstroms.

9. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The average pore size variation gradient of the degassing membrane is 0.2-6 nm / μm, and the water contact angle of the outer surface is at least greater than 100°; The average pore size variation gradient of the degassing membrane is calculated as follows: (SEM average pore size of the degassing pores inside the degassing membrane - SEM average pore size of the outer surface of the degassing membrane) / average thickness of the degassing membrane.

10. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The outer surface is a dense surface, and the porosity of the outer surface is less than 1%. The O2 permeation rate of the degassing membrane is 10-40 L / (min·bar·0.1m). 2 ).

11. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The outer surface has several silver-like cracks, the SEM width of the cracks is no more than 20 nm, and the average SEM length of the cracks is 10-90 nm.

12. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The outer surface has an external degassing region and an external dense region. The porosity of the external dense region is less than 1%. The external degassing region contains a plurality of external degassing pores. The average SEM pore size of the external degassing pores in the external degassing region is 10-90 nm, and the density of the external degassing pores is 10-80 pores / μm. 2 ; The O2 permeation rate of the degassing membrane is 35-80 L / (min·bar·0.1m). 2 ).

13. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The outer surface has a plurality of uniformly distributed external degassing pores, the SEM average pore diameter of which is 10-90 nm, and the density of which is 1-30 pores / 10 μm. 2 ; The O2 permeation rate of the degassing membrane is 30-60 L / (min·bar·0.1m). 2 ).

14. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The main body comprises a skin layer and a support layer. One side of the support layer is an inner surface, and one side of the skin layer is an outer surface. The other side of the skin layer and the other side of the support layer transition with continuous fibers. The thickness of the skin layer is 0.1-3 μm. The support layer contains porous fibers for forming a porous structure. The average SEM diameter of the porous fibers is 10-120 nm, and the density of the porous fibers is 30-450 fibers / μm. 2 .

15. The asymmetric polypropylene hollow fiber degassing membrane according to claim 1, characterized in that: The CO2 permeation rate of the degassing membrane is 10-90 L / (min·bar·0.1m). 2 ); The deoxygenation efficiency of the degassing membrane is greater than or equal to 90%; The tensile strength of the degassing membrane is not less than 200 CN, and the elongation at break is 50-500%.

16. The preparation process of an asymmetric polypropylene hollow fiber degassing membrane according to any one of claims 1-15, characterized in that, The process includes the following steps: S1, spinning, where PP material is melted and extruded through a die, forming a molded product with a hollow inner cavity under the action of an inert gas as the core liquid; wherein the die extrusion temperature is at least greater than 210°C; The weight-average molecular weight of PP material is 100,000-800,000, the molecular weight distribution index is 1.5-7, and the isotacticity of PP material is not less than 95%. S2, Pre-crystallization: The molded product is placed in an air section for pre-crystallization, where the temperature of the air section is 30-120℃ and the pre-crystallization time is 0.05-0.6s. The inert gas flow rate is 0.5-4 ml / min, the temperature of the inert gas in the air section is 80-130℃, and the temperature of the inert gas in the air section is higher than the ambient temperature of the air section. S3, air-cooled crystallization: the molded product obtained in step S2 is cooled by blowing air to obtain nascent fibers, wherein the blowing temperature is 30-70℃ and the blowing speed is 20-100m / min; S4, one-time heat setting, involves the first heat setting treatment of the nascent fibers to obtain a heat-set semi-finished product; S5, cold drawing to form holes, the heat-set semi-finished product is cold drawn, wherein the ratio of the cold drawing temperature to the temperature of the inert gas in the air section satisfies 1:(2.5-6), and the cold-drawn semi-finished product is obtained; S6, hot drawing to expand the hole, the cold-drawn semi-finished product is hot drawn to expand the hole, wherein the ratio of the hot drawing temperature to the cold drawing temperature satisfies (3-7):1, and the hot-drawn semi-finished product is obtained; S7, Secondary heat setting: The hot-drawn semi-finished product undergoes a second heat setting process to obtain a hollow fiber degassed membrane.

17. The preparation process of an asymmetric polypropylene hollow fiber degassing membrane according to claim 16, characterized in that, In step S1, the melting process includes melting, mixing and metering steps. The metering temperature is 2-10℃ higher than the die extrusion temperature. The die extrusion temperature is 215-230℃ and the length-to-diameter ratio of the die is 2-6.

18. The preparation process of an asymmetric polypropylene hollow fiber degassing membrane according to claim 16, characterized in that, In step S4, the heat-set semi-finished product is slightly stretched with an elongation of 0.5-3%. The temperature of the first heat setting is 120-150℃, and the time of the first heat setting is 60-150 min. In step S7, the second heat setting temperature is 10-30°C higher than the first heat setting temperature, and the second heat setting time is 0.5-3 minutes.

19. The preparation process of an asymmetric polypropylene hollow fiber degassing membrane according to claim 16, characterized in that, In step S5, the cold drawing elongation rate is 20%-40%, and the cold drawing rate is 10-30% / min; In step S6, the hot stretching elongation is 80%-120%, and the hot stretching rate is 0.3-1.3% / min.

20. The application of an asymmetric polypropylene hollow fiber degassing membrane according to any one of claims 1-15, characterized in that, The degassing membrane is used for degassing ultrapure water.

Citation Information

Patent Citations

  • Asymmetric hollow fiber membranes and methods of making and using same

    CN113226525A

  • Preparation of membrane

    JP1986101206A

  • Polyolefin hollow fiber membrane for asymmetric degassing as well as preparation method and application of polyolefin hollow fiber membrane

    CN115155329A