A self-healing gel polymer electrolyte and its preparation method and application, polymer lithium battery
By using self-healing gel polymer electrolytes in lithium-ion batteries, the problem of cracks and fractures in solid-state batteries under external force is solved, the transmission efficiency and conductivity of lithium ions are improved, and the electrochemical performance and conductivity of lithium-ion batteries are improved. Cycling stability.
Patent Information
- Application Number
- CN202311811099.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-12-26
AI Technical Summary
The polymer electrolyte of solid-state lithium-ion batteries is prone to micro-cracks and fractures when subjected to external forces, resulting in obstruction of the transmission of lithium ions, affecting battery performance and cycle life, and its ionic conductivity is low, limiting its application.
A self-healing gel polymer electrolyte is used by combining ionic liquid, poly(ethylene glycol) methacrylate, 1-methyl-3-(4-vinylbenzyl)-1hydro-imidazole-3-ium Materials such as bis(trifluoromethyl)sulfonimide salt and lithium salt are mixed and thermally polymerized and solidified into a gel state to form an electrolyte with self-healing ability and increase the lithium ion migration number and conductivity.
A self-healing gel polymer electrolyte with high conductivity and stable interface contact at room temperature has been achieved, which improves the electrochemical performance and cycle performance of lithium-ion batteries, and enhances the rate performance and stability of lithium batteries.
Smart Images

Figure CN117895067B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytes, and in particular relates to a self-healing gel polymer electrolyte, a preparation method and application thereof, and a polymer lithium battery. Background Art
[0002] With the continuous progress of human society, people's demand for energy is growing. However, behind the rapid development, we have to face urgent problems such as the depletion of fossil energy and the worsening of environmental pollution. In the past few decades, although lithium-ion batteries have been recognized as an old-fashioned power source option, a series of safety issues such as fire and explosion caused by electrolyte leakage have become an obstacle to the continued use of lithium-ion batteries. Therefore, people have an increasing demand for lithium-ion batteries with safety, high energy density and long cycle life. At this stage, replacing traditional lithium-ion batteries using liquid electrolytes with all-solid-state batteries using solid electrolytes is seen as an effective way to solve safety problems.
[0003] Solid electrolytes are divided into inorganic solid electrolytes and solid polymer electrolytes. Among them, polymer electrolytes are composed of polymer skeletons containing polar functional groups and lithium salts. Compared with liquid electrolytes, they have the advantages of inhibiting lithium dendrites, easy preparation, stability to metallic lithium, and no leakage and flatulence. However, as a key component of flexible lithium batteries, solid electrolytes are inevitably subjected to external forces such as stretching, twisting and bending in practical applications, which lead to microcracks and fractures, hinder the transmission of lithium ions inside the solid electrolyte, and seriously affect the performance and cycle performance of solid electrolyte batteries. In addition, the increase in the crystalline phase in the polymer electrolyte causes a significant decrease in its ionic conductivity, and the lithium ion migration number is low, basically around 0.2, which limits its application. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a self-healing gel polymer electrolyte and its preparation method and application, and a polymer lithium battery. The self-healing gel polymer electrolyte provided by the present invention has high conductivity at room temperature, stable interface contact and can achieve self-healing without external stimulation.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a self-healing gel polymer electrolyte, which comprises the following preparation raw materials in parts by mass:
[0007] 2 to 12 parts of ionic liquid,
[0008] 10 to 100 parts of poly(ethylene glycol) methacrylate,
[0009] 0.5 to 18 parts of 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt,
[0010] 2 to 33 parts of lithium salt,
[0011] Thermal initiator 0.02-0.3 parts.
[0012] Preferably, the ionic liquid includes one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hexyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 2,3-dimethyl-1-propylimidazolium bis(trifluoromethanesulfonyl)imide, 1-butyl-1-methylpiperidinium bis(trifluoromethanesulfonyl)imide and 1-octyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
[0013] Preferably, the thermal initiator comprises an azo initiator and / or an organic peroxide.
[0014] Preferably, the lithium salt includes one or more of LiPF6, LiClO4, LiTFSI, LiFSI, LiBOB and LiDFOB.
[0015] Preferably, the relative molecular weight of the poly(ethylene glycol) methacrylate is 400 to 4000 g / mol.
[0016] The present invention also provides a method for preparing the self-healing gel polymer electrolyte described in the above technical solution, comprising the following steps:
[0017] The ionic liquid, poly(ethylene glycol) methacrylate, 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, lithium salt and thermal initiator are mixed to obtain a precursor solution;
[0018] The precursor solution is thermally polymerized and solidified into a gel state to obtain a self-healing gel polymer electrolyte.
[0019] Preferably, the temperature of the thermal polymerization curing is 40 to 120° C. and the time is 4 to 12 hours.
[0020] The present invention also provides the use of the self-healing gel polymer electrolyte described in the above technical solution or the self-healing gel polymer electrolyte prepared by the preparation method described in the above technical solution in a polymer lithium battery.
[0021] The present invention also provides a polymer lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte, characterized in that the solid electrolyte is the self-healing gel polymer electrolyte described in the above technical solution or the self-healing gel polymer electrolyte prepared by the preparation method described in the above technical solution.
[0022] Preferably, the positive electrode comprises a positive electrode active material, a current collector, a conductive agent and a binder; the mass ratio of the positive electrode active material, the conductive agent and the binder is 8:1:1.
[0023] The present invention provides a self-healing gel polymer electrolyte, which comprises the following raw materials by weight: 2 to 12 parts of ionic liquid, 10 to 100 parts of poly(ethylene glycol) methacrylate, 0.5 to 18 parts of 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, 2 to 33 parts of lithium salt, and 0.02 to 0.3 parts of thermal initiator. The two imidazolium cations in the self-healing electrolyte react with one anion (TFSI - ) have a strong interaction, which makes poly(ethylene glycol) methacrylate have good self-healing properties; at the same time, sufficient imidazolium cations will attract TFSI- in large quantities, releasing Li + , the prepared self-healing electrolyte has a high lithium ion migration number and conductivity, thereby improving the electrochemical performance of lithium-ion batteries; ionic liquids have good ion transport properties, which can improve the conductivity of polymer electrolytes at room temperature without reducing mechanical properties, and polymer electrolytes are flexible and can have good contact with the interface, so the polymer electrolyte has good interfacial compatibility with the lithium metal negative electrode, reducing the impedance of the interface, thereby improving the cycle performance and rate performance of the lithium battery. In summary, the polymer electrolyte provided by the present invention has high conductivity at room temperature, stable interfacial contact, and can achieve self-healing without external stimulation. According to the test results of Example 1, the self-healing gel polymer electrolyte provided by the present invention has an ionic conductivity of 1.32×10 -4 S cm -1 , the lithium ion migration number is 0.59, the electrochemical window is 5.2V, and the prepared lithium ion battery has excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The physical picture and SEM picture of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention;
[0025] Figure 2 This is a lithium ion migration graph of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention;
[0026] Figure 3 This is an electrochemical window diagram of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention;
[0027] Figure 4 This is a thermogravimetric diagram of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention;
[0028] Figure 5This is a cycle stability curve of a Li / / Li symmetric button cell assembled with a self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention;
[0029] Figure 6 This is a diagram of the self-healing process of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention at room temperature. DETAILED DESCRIPTION
[0030] The present invention provides a self-healing gel polymer electrolyte, which comprises the following preparation raw materials in parts by mass:
[0031] 2 to 12 parts of ionic liquid,
[0032] 10 to 100 parts of poly(ethylene glycol) methacrylate,
[0033] 0.5 to 18 parts of 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt,
[0034] 2 to 33 parts of lithium salt,
[0035] Thermal initiator 0.02-0.3 parts.
[0036] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used, and commercially available products known to those skilled in the art may be used.
[0037] The self-healing gel polymer electrolyte provided by the present invention comprises the following preparation raw materials, calculated by weight: 2 to 12 parts of ionic liquid, preferably 3 to 10 parts.
[0038] In the present invention, the ionic liquid preferably includes one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hexyl-3-methylimidazolium tetrafluoroboric acid, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 2,3-dimethyl-1-propylimidazolium bis(trifluoromethanesulfonyl)imide, 1-butyl-1-methylpiperidinium bis(trifluoromethanesulfonyl)imide and 1-octyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, more preferably 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. When the ionic liquid is the above-mentioned ionic liquid, the present invention has no special restrictions on the ratio of different types of ionic liquids, and any ratio can be used.
[0039] In the present invention, the ionic liquid accelerates the transmission of lithium ions, improves the conductivity of the polymer electrolyte at room temperature without reducing the mechanical properties, and the polymer electrolyte has good interface compatibility with the lithium metal negative electrode, reduces the impedance of the interface, thereby improving the cycle performance and rate performance of the lithium battery.
[0040] Based on 1 mass part of the ionic liquid, the raw materials for preparing the self-healing gel polymer electrolyte provided by the present invention include 10 to 100 parts of poly(ethylene glycol) methacrylate, preferably 45 to 65 parts, and more preferably 50 to 60 parts.
[0041] In the present invention, the relative molecular weight of the poly(ethylene glycol) methacrylate is preferably 400 to 4000 g / mol, more preferably 450 to 1000 g / mol. In the present invention, the function of the poly(ethylene glycol) methacrylate is to transport lithium ions.
[0042] Based on 1 mass part of the ionic liquid, the raw materials for preparing the self-healing gel polymer electrolyte provided by the present invention include 0.5 to 18 parts of 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, preferably 2 to 8 parts, and more preferably 4 to 6 parts.
[0043] In the present invention, the preparation method of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt preferably comprises the following steps:
[0044] Mixing 4-vinylbenzyl chloride, 1-methylimidazole and a first solvent, and performing a substitution reaction to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride;
[0045] The 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride and lithium bis(trifluoromethanesulfonyl)imide are mixed to carry out an ion exchange reaction to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt.
[0046] In the present invention, 4-vinylbenzyl chloride, 1-methylimidazole and the first solvent are preferably mixed to carry out a substitution reaction to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride.
[0047] In the present invention, the structural formula of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride is as follows:
[0048] In the present invention, the molar ratio of 4-vinylbenzyl chloride to 1-methylimidazole is preferably (1-3):1, more preferably 1:1; the first solvent is preferably acetonitrile. The present invention has no particular limitation on the amount of the first solvent, as long as it can fully dissolve each component.
[0049] In the present invention, 4-vinylbenzyl chloride, 1-methylimidazole and the first solvent are preferably mixed in the following manner: the mixture obtained by mixing 4-vinylbenzyl chloride and the first solvent is heated, and then 1-methylimidazole is added dropwise to the heated mixture; the heating temperature is preferably 20 to 80° C., more preferably 40 to 60° C.; the dropping speed is preferably 1 to 10 mL / h, more preferably 3 to 5 mL / h. The present invention adopts the method of adding 1-methylimidazole dropwise to avoid violent heat release during the reaction and intensify the side reaction.
[0050] In the present invention, the temperature of the substitution reaction is preferably 20-80°C, more preferably 40-60°C; the time of the substitution reaction is preferably 12-200h, more preferably 30-96h; the substitution reaction is preferably carried out under stirring; the stirring rate is preferably 200-500rpm, more preferably 350rpm; the substitution reaction is preferably timed from the completion of the dropwise addition.
[0051] After the substitution reaction is completed, the present invention preferably further comprises: subjecting the substitution reaction product to a first desolventizing, washing, and a second desolventizing in sequence to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazol-3-ium chloride. In the present invention, the first desolventizing is preferably carried out by rotary evaporation; the temperature of the rotary evaporation is preferably 30 to 100°C, more preferably 50 to 70°C; the time of the rotary evaporation is preferably 10 to 100 minutes, more preferably 30 to 50 minutes; the washing is preferably carried out with ethyl acetate; the second desolventizing is preferably carried out by rotary evaporation; the temperature of the rotary evaporation is preferably 30 to 100°C, more preferably 50 to 70°C; the time of the rotary evaporation is preferably 10 to 100 minutes, more preferably 30 to 50 minutes. In the present invention, the first desolventizing removes the solvent used for the substitution reaction, and the second desolventizing removes the detergent used for washing.
[0052] After obtaining the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride, the present invention mixes the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride and lithium bis(trifluoromethanesulfonyl)imide to carry out an ion replacement reaction to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt.
[0053] In the present invention, the ion exchange reaction of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride and lithium bis(trifluoromethanesulfonyl)imide is preferably carried out by mixing an aqueous solution of 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride, an aqueous solution of lithium bis(trifluoromethanesulfonyl)imide and dichloromethane for a first ion exchange reaction, standing and stratifying, and washing the obtained organic layer with an aqueous solution of lithium bis(trifluoromethanesulfonyl)imide for multiple times to carry out a second ion exchange reaction to obtain an ion exchange reaction product.
[0054] In the present invention, the molar ratio of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride to lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is preferably (1-3):1, more preferably (1-2):1; the concentration of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride in the aqueous solution of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride is preferably 5-10 mol / L, more preferably 6-8 mol / L; the volume ratio of the aqueous solution of the 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride to dichloromethane is preferably (2-4):1, more preferably 2:1; the first ion is placed The temperature of the exchange reaction is preferably 20-30°C, more preferably 25°C; the time of the first ion exchange reaction is preferably 10-20 min, more preferably 15 min; the concentration of lithium bistrifluoromethanesulfonyl imide in the aqueous solution of lithium bistrifluoromethanesulfonyl imide is preferably 1-5 mol / L, more preferably 2-4 mol / L; the volume ratio of the organic layer to the aqueous solution of lithium bistrifluoromethanesulfonyl imide is preferably (2-4):1, more preferably 2:1; the temperature of the second ion exchange reaction is preferably 20-30°C, more preferably 25°C; the time of the second ion exchange reaction is preferably 10-20 min, more preferably 15 min; the number of washings is preferably 2-8 times, more preferably 3-6 times.
[0055] In the present invention, 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride is first dissolved in distilled water, and then replaced with a large amount of lithium bistrifluoromethanesulfonyl imide (LiTFSI), and then replaced with LiTFSI in small amounts and multiple times.
[0056] After the substitution reaction is completed, the present invention preferably further comprises: subjecting the substitution reaction product to vacuum distillation and drying in sequence to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt. In the present invention, the pressure of the vacuum distillation is preferably 100-200 Pa, more preferably 110-150 Pa; the temperature of the vacuum distillation is preferably 20-120° C., more preferably 50-70° C.; the time of the vacuum distillation is preferably 10-100 min, more preferably 30-50 min; the temperature of the drying is preferably 20-120° C., more preferably 60-100° C.; the time of the drying is preferably 10-100 h, more preferably 24-50 h; the drying is preferably vacuum drying; the vacuum degree of the vacuum drying is preferably 20-100 Pa, more preferably 50 Pa.
[0057] In the present invention, the two imidazolium cations on the polymer chain have a strong interaction with an anion at the same time, so that the electrolyte membrane can achieve self-healing at room temperature without external stimulation.
[0058] Based on 1 mass part of the ionic liquid, the raw materials for preparing the self-healing gel polymer electrolyte provided by the present invention include 2 to 33 parts of lithium salt, preferably 5 to 28 parts, and more preferably 10 to 26 parts. In the present invention, the lithium salt preferably includes one or more of LiPF6, LiClO4, LiTFSI, LiFSI, LiBOB and LiDFOB, more preferably LiTFSI. When the lithium salt is the above-mentioned types, the present invention has no special restrictions on the ratio of different types of lithium salts, and any ratio is sufficient. In the present invention, the function of the lithium salt is to provide lithium ions.
[0059] Based on 1 mass part of the ionic liquid, the raw materials for preparing the self-healing gel polymer electrolyte provided by the present invention include 0.02 to 0.3 parts of thermal initiator, preferably 0.05 to 0.2 parts. In the present invention, the thermal initiator preferably includes an azo initiator and / or an organic peroxide, more preferably an azo initiator; the azo initiator preferably includes azobisisobutyronitrile and / or azobisisoheptanenitrile, more preferably azobisisobutyronitrile (AIBN); the organic peroxide preferably includes benzoyl peroxide and / or tert-butyl perbenzoate, more preferably benzoyl peroxide. When the thermal initiator is the above-mentioned types, the present invention has no special restrictions on the ratio of different types of thermal initiators, and any ratio can be used.
[0060] In the present invention, the self-healing gel polymer electrolyte is preferably a self-healing gel polymer electrolyte membrane, and the thickness of the self-healing gel polymer electrolyte membrane is preferably 100 to 200 μm, more preferably 120 to 150 μm.
[0061] The present invention also provides a method for preparing the self-healing gel polymer electrolyte described in the above technical solution, comprising the following steps:
[0062] The ionic liquid, poly(ethylene glycol) methacrylate, 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, lithium salt and thermal initiator are mixed to obtain a precursor solution;
[0063] The precursor solution is thermally polymerized and solidified into a gel state to obtain a self-healing gel polymer electrolyte.
[0064] The invention mixes ionic liquid, poly(ethylene glycol) methacrylate, 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, lithium salt and thermal initiator to obtain a precursor solution.
[0065] In the present invention, the mixing is preferably: first mixing the ionic liquid, poly (ethylene glycol) methacrylate, 1-methyl-3- (4-vinylbenzyl) -1 hydrogen-imidazol-3-ium bis (trifluoromethyl) sulfonyl imide salt and lithium salt to obtain a first mixture; second mixing the first mixture and thermal initiator to obtain a precursor solution. In the present invention, the first mixing and the second mixing are independently carried out under stirring conditions; the stirring rate is preferably 20 to 200 rpm, more preferably 100 rpm; the temperature of the first mixing is preferably 20 to 80°C, more preferably 40°C; the time of the first mixing is preferably 0.5 to 200h, more preferably 0.5 to 96h; the temperature of the second mixing is preferably 10 to 100°C, more preferably 30 to 40°C; the time of the second mixing is preferably 4 to 12h, more preferably 6 to 10h.
[0066] In the present invention, the temperature of the thermal polymerization curing is preferably 10-100°C, more preferably 50-70°C, and the time is preferably 4-12h, more preferably 6-10h; the thermal polymerization curing is preferably carried out under vacuum conditions; the vacuum degree of the vacuum conditions is preferably 20-100Pa, more preferably 50Pa.
[0067] In the present invention, the precursor solution is preferably cured into a gel state by thermal polymerization. After the precursor solution is formed into a film on the surface of a substrate, it is thermally cured into a gel state. The film formation is preferably film formation by scraping. The equipment used for the film formation by scraping is preferably a scraper. The scraper is preferably a scraper with a 750 μm groove. The substrate is preferably a plastic film.
[0068] After the thermal polymerization is cured into a gel state, the present invention preferably separates the gel film obtained by the thermal polymerization from the substrate to obtain a self-healing gel polymer electrolyte membrane.
[0069] The specific reaction process of the self-healing gel polymer electrolyte membrane in the present invention is as follows:
[0070]
[0071] The present invention also provides the use of the self-healing gel polymer electrolyte described in the above technical solution or the self-healing gel polymer electrolyte prepared by the preparation method described in the above technical solution in a polymer lithium battery.
[0072] The present invention also provides a polymer lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte, wherein the solid electrolyte is the self-healing gel polymer electrolyte described in the above technical solution or the self-healing gel polymer electrolyte prepared by the preparation method described in the above technical solution.
[0073] In the present invention, the positive electrode preferably includes a positive electrode active material, a current collector, a conductive agent and a binder; the mass ratio of the positive electrode active material, the conductive agent and the binder is preferably 8:1:1; the positive electrode active material preferably includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and lithium iron manganese phosphate, more preferably lithium iron phosphate; the current collector preferably includes copper foil or aluminum foil, more preferably aluminum foil; the conductive agent preferably includes one or more of acetylene black, Ketjen black and carbon nanotubes, more preferably acetylene black; the binder preferably includes one or more of polytetrafluoroethylene, polyurethane and polyvinylidene fluoride, more preferably polyvinylidene fluoride; the negative electrode is preferably metallic lithium. The present invention has no special requirements for the assembly method of the polymer lithium battery, and the assembly method familiar to those skilled in the art can be used.
[0074] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0075] Example 1
[0076] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0077] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0078] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.056 g, 0.118 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 100 rpm for 30 min at 40 °C to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 100 rpm for 6 h at 40 °C to obtain a uniform precursor solution;
[0079] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa vacuum and 70° C. for 6 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0080] Example 2
[0081] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0082] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0083] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.0263 g, 0.055 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 100 rpm for 30 min at 40 °C to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 100 rpm for 6 h at 40 °C to obtain a uniform precursor solution;
[0084] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa and 70° C. for 12 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0085] The film-forming property of the self-healing gel polymer electrolyte membrane prepared in Example 2 is worse than that of the self-healing gel polymer electrolyte membrane prepared in Example 1.
[0086] Example 3
[0087] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0088] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0089] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.088 g, 0.184 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 40°C at 100 rpm for 30 min to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 40°C at 100 rpm for 6 h to obtain a uniform precursor solution;
[0090] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa and 70° C. for 12 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0091] The film-forming property of the self-healing gel polymer electrolyte membrane prepared in Example 3 is worse than that of the self-healing gel polymer electrolyte membrane prepared in Example 1.
[0092] Example 4
[0093] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0094] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0095] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.056 g, 0.118 mmol), lithium salt (LiTFSI, 0.122 g, 0.425 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 40° C. and 100 rpm for 30 min to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 40° C. and 100 rpm for 6 h to obtain a uniform precursor solution;
[0096] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa and 70° C. for 12 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0097] Example 5
[0098] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0099] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0100] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.056 g, 0.118 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 100 rpm for 30 min at 40 °C to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 100 rpm for 6 h at 40 °C to obtain a uniform precursor solution;
[0101] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa vacuum and 70° C. for 4 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0102] Example 6
[0103] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0104] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0105] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.056 g, 0.118 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 100 rpm for 30 min at 40 °C to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 100 rpm for 6 h at 40 °C to obtain a uniform precursor solution;
[0106] The precursor solution was coated onto the surface of the plastic film with a 750 μm thick scraper, and then thermally cured in a vacuum oven at 50 Pa vacuum and 70° C. for 8 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0107] Example 7
[0108] 4-vinylbenzyl chloride (2.41 mL, 31 mmol) and anhydrous acetonitrile (25 mL) were placed in a three-necked flask equipped with a constant pressure dropping funnel, 1-methylimidazole (4.29 mL, 31 mmol) was added to the constant pressure dropping funnel, the solution in the three-necked flask was heated to 40°C, 1-methylimidazole (4.29 mL, 31 mmol) was slowly added dropwise from the constant pressure dropping funnel at a rate of 5 mL / h, after the dropwise addition was completed, the solution was stirred at a rate of 350 rpm for 96 h to carry out a substitution reaction, after the reaction was completed, the solvent was removed by rotary evaporation at a rotary evaporation temperature of 70°C for 30 min, impurities were washed off with ethyl acetate, and the rotary evaporation was repeated at a rotary evaporation temperature of 70°C for 30 min to obtain 1-methyl-3-(4-vinylbenzyl)-1 hydrogen-imidazole-3-ium chloride;
[0109] 1-Methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium chloride (4 g, 16.8 mmol) was dissolved in distilled water and transferred to a separation funnel, dichloromethane (DCM, 20 mL) was added, and then LiTFSI (4.92 g, 17.14 mmol) solution was added and shaken at 25°C and allowed to stand for ion replacement for 20 min, and then the organic layer was separated and washed with H2O (2 mL) added with LiTFSI (0.1 g, 0.348 mmol) solution at 25°C for ion replacement for 15 min, and the washing was repeated 4 times. The organic layer was evaporated under reduced pressure at a pressure of 110 Pa, a temperature of 70°C, and a time of 30 min, and then dried under vacuum at a vacuum degree of 50 Pa, a drying temperature of 60°C, and a drying time of 24 h to obtain 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt;
[0110] Poly(ethylene glycol) methyl ether methacrylate (0.5 g, 0.526 mmol), 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt (0.056 g, 0.118 mmol), lithium salt (LiTFSI, 0.163 g, 0.568 mmol) and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl imide salt) (0.056 g, 0.142 mmol) were placed in a 2.5 mL vial, stirred at 100 rpm for 30 min at 40 °C to dissolve, and then a thermal initiator (AIBN, 0.001438 g, 0.00876 mmol) was added and stirred at 100 rpm for 6 h at 40 °C to obtain a uniform precursor solution;
[0111] The precursor solution was coated onto the surface of the plastic film using a scraper with a groove of 750 μm, and then thermally cured in a vacuum oven at 50 Pa and 70° C. for 12 h, and then the film was peeled off to obtain a self-healing gel polymer electrolyte membrane.
[0112] Performance Testing
[0113] (1) The self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention was scanned by electron microscope. The results are as follows: Figure 1 shown.
[0114] Depend on Figure 1 It can be seen that the self-healing gel polymer electrolyte prepared in Example 1 is a transparent self-supporting electrolyte membrane. The overall morphology shows that the electrolyte membrane has excellent mechanical flexibility and is dense and non-porous at the microscopic level, which is conducive to the interface contact between the electrodes.
[0115] (2) The lithium ion migration number of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention was tested. The results are as follows: Figure 2 shown.
[0116] Depend on Figure 2 It can be seen that the Bruce-Vincent-Evans equation is used to calculate the lithium ion migration number. Sufficient imidazolium cations will attract TFSI- in large quantities, releasing Li + , which increases the number of lithium ion migration.
[0117] (3) The electrochemical window of the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention was tested, specifically by cyclic voltammetry in a two-electrode battery at 0.1 mVs -1 The electrochemical stability window was measured at a scan rate of Figure 3 shown.
[0118] Depend on Figure 3 It can be seen that the self-healing electrolyte has excellent stability.
[0119] (4) The self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention was tested by thermogravimetric analysis, specifically: thermogravimetric analysis is a method for measuring the relationship between the weight loss of a sample and the temperature. The temperature was raised at a constant rate of 10° C. min -1 , 100mLmin -1 Under nitrogen flow, the test temperature was within the range of 25-600℃, and the thermal stability and weight loss of the solid polymer electrolyte membrane were analyzed. Figure 4 shown.
[0120] Depend on Figure 4 It can be seen that the self-healing polymer electrolyte provided by the present invention does not undergo thermal decomposition below 300° C., indicating that the self-healing polymer electrolyte has good thermal stability.
[0121] (5) The cycle stability of the Li / / Li symmetric button cell assembled with the self-healing gel polymer electrolyte membrane prepared in Example 1 of the present invention was tested. The results are as follows: Figure 5 shown.
[0122] Depend on Figure 5 It can be seen that the voltage remains constant after 400 h of cycling, indicating that the interface between the Li negative electrode and the self-healing electrolyte is relatively stable. This result shows that the self-healing electrolyte has excellent compatibility with the Li negative electrode and good ability to inhibit lithium dendrites.
[0123] (6) The self-healing of the self-healing gel polymer electrolyte membrane prepared in Examples 1 to 3 of the present invention at room temperature was tested. The specific process was as follows: the membrane was cut into two pieces with a scalpel, the two separated parts were brought into contact, and the membrane was left to stand for 2 hours. The healing of the membrane was observed. The prepared self-healing electrolyte was cut into two pieces with a scalpel, and then combined together. The healing was carried out for 30 minutes. The self-healed electrolyte was able to lift a 20g weight. The healing results of the self-healing gel polymer electrolyte membrane prepared in Example 1 are shown in FIG. Figure 6 shown.
[0124] Depend on Figure 6 It can be seen that the self-healing gel polymer electrolyte membrane prepared in Example 1 is healed after cutting. Although the gap is not completely eliminated, the healed membrane can withstand a weight of 20g without breaking. It shows good self-healing performance. The self-healing gel polymer electrolyte membranes prepared in Examples 2 to 3 have worse self-healing properties than the self-healing gel polymer electrolyte membrane prepared in Example 1.
[0125] (7) The room temperature conductivity of the self-healing gel polymer electrolyte membranes prepared in Examples 4 to 7 was tested. The results are shown in Table 1.
[0126] Table 1 Room temperature conductivity of self-healing gel polymer electrolyte membrane
[0127] Serial number <![CDATA[Room temperature conductivity (S·cm -1 )]]> Example 4 <![CDATA[2.28×10 -5 ]]> Example 5 <![CDATA[3.52×10 -5 ]]> Example 6 <![CDATA[1.56×10 -5 ]]> Example 7 <![CDATA[1.02×10 -5 ]]>
[0128] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A self-healing gel polymer electrolyte, characterized in that: The preparation includes the following raw materials by weight: 2 to 12 parts of an ionic liquid, wherein the ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; 10 to 100 parts of poly(ethylene glycol) methacrylate, 0.5 to 18 parts of 1-methyl-3-(4-vinylbenzyl)-1-hydrogen-imidazol-3-ium bis(trifluoromethyl)sulfonyl imide salt, 2~33 parts of lithium salt, Thermal initiator 0.02~0.3 parts.
2. The self-healing gel polymer electrolyte according to claim 1, characterized in that: The thermal initiator includes an azo initiator and / or an organic peroxide.
3. The self-healing gel polymer electrolyte according to claim 1, characterized in that: The lithium salt includes one or more of LiPF6, LiClO4, LiTFSI, LiFSI, LiBOB and LiDFOB.
4. The self-healing gel polymer electrolyte according to claim 1, characterized in that: The relative molecular weight of the poly(ethylene glycol) methacrylate is 400-4000 g / mol.
5. The method for preparing the self-healing gel polymer electrolyte according to any one of claims 1 to 4, characterized in that: The following steps are involved: The ionic liquid, poly (ethylene glycol) methacrylate, 1-methyl-3- (4-vinylbenzyl) -1-hydrogen-imidazol-3-ium bis (trifluoromethyl) sulfonyl imide salt, lithium salt and thermal initiator are mixed to obtain a precursor solution; the ionic liquid is 1-ethyl-3-methylimidazolium bis (trifluoromethyl) sulfonyl imide salt; The precursor solution is thermally polymerized and solidified into a gel state to obtain a self-healing gel polymer electrolyte.
6. The preparation method according to claim 5, characterized in that: The temperature of the thermal polymerization curing is 40-120° C. and the time is 4-12 hours.
7. Use of the self-healing gel polymer electrolyte according to any one of claims 1 to 4 or the self-healing gel polymer electrolyte prepared by the preparation method according to claim 5 or 6 in a polymer lithium battery.
8. A polymer lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte, characterized in that: The solid electrolyte is the self-healing gel polymer electrolyte described in any one of claims 1 to 4 or the self-healing gel polymer electrolyte prepared by the preparation method described in claim 5 or 6.
9. The polymer lithium battery according to claim 8, characterized in that: The positive electrode comprises a positive electrode active material, a current collector, a conductive agent and a binder; the mass ratio of the positive electrode active material, the conductive agent and the binder is 8:1:1.
Citation Information
Patent Citations
Cross-linking polymerization method for preparing solid electrolyte of polyionic liquid
CN109608592A
In-situ prepared POSS ionic gel polymer electrolyte and preparation method thereof
CN111900466A
Self-healing network polymer electrolyte, preparation method and application thereof, and polymer lithium battery
CN115954539A
Poly(ionic liquid)s as new materials for co2 separation and other applications
US20090266230A1
In-situ preparation and application of solid polymer electrolyte
WO2023109659A1