A kind of fast-hardening high-strength steel fiber reinforced concrete and preparation method thereof

By optimizing the proportion of concrete raw materials and internal curing mechanism, combined with the use of steel fiber and water-reducing agent, the problem of uneven structure and cracking of fast-hardening concrete has been solved, and high-strength, low-cost fast-hardening steel fiber reinforced concrete has been achieved, which is suitable for Emergency repairs and bridge projects.

CN117902874BActive Publication Date: 2024-10-08GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410080655.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-08
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

Rapidly hardening concrete is prone to uneven internal structure, expansion, and honeycomb pitting after using early-strength additives, leading to later cracking and reduced strength. The cost is high and it is difficult to reduce the amount of cement.

Method used

Using the optimized ratio of sulphoaluminate cement, Portland cement, gypsum, quartz sand, bauxite, silica fume, heavy calcium powder and steel fiber, through chemical reaction, filling gaps and internal curing mechanism, combined with steel The bridging effect of fibers and the use of polycarboxylate superplasticizer form high-strength, low-expansion concrete.

Benefits of technology

Significantly reduces the risk of concrete cracking, improves compressive strength and workability, reduces cement consumption and production costs, and improves the long-term strength and durability of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117902874B_ABST
    Figure CN117902874B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of concrete, and in particular to a fast-hardening high-strength steel fiber reinforced concrete and a preparation method thereof. A fast-hardening high-strength steel fiber reinforced concrete, in terms of mass fraction, comprises raw materials for preparation: 450-530 parts of sulphoaluminate cement, 150-180 parts of Portland cement, 134-198 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 20-67 parts of heavy calcium powder, 134-217 parts of steel fiber, 23-67 parts of water reducer, and 204-331 parts of water; the above scheme reduces the risk of concrete cracking, improves the strength of concrete, and reduces the amount of cement used, thereby reducing the production cost of concrete, through the synergistic effect of sulphoaluminate cement, Portland cement, gypsum, quartz sand, bauxite, silica fume, heavy calcium powder, steel fiber, water reducer and water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, and in particular to a fast-hardening high-strength steel fiber reinforced concrete and a preparation method thereof. Background Art

[0002] Rapid-hardening concrete is widely used in emergency construction or crack repair due to its extremely fast setting speed, high early strength, good frost resistance and excellent adhesion. When preparing rapid-hardening concrete, early strength agents are often added to promote cement hydration, thereby achieving the goal of accelerating the early strength development of concrete. However, after using early strength agents, the internal structure of the concrete is uneven and not dense, which will produce a certain amount of expansion, and the surface of the concrete is prone to honeycomb pockmarks, making the concrete prone to cracking and deformation in the later stage. At the same time, the uneven internal structure will also reduce the long-term strength of the concrete.

[0003] In summary, in the process of configuring rapid-hardening concrete, reducing the risk of concrete cracking, improving concrete strength, reducing cement consumption and saving costs have become issues that need to be urgently addressed. Summary of the invention

[0004] In view of this, the present invention provides a rapid-hardening high-strength steel fiber reinforced concrete and a preparation method thereof, which are used to solve the technical problems of high cracking risk, low concrete strength and high cost of existing rapid-hardening concrete.

[0005] The first aspect of the present invention provides a fast-hardening high-strength steel fiber reinforced concrete, wherein the raw materials for preparation include, by weight:

[0006] 450-530 parts of sulphoaluminate cement, 150-180 parts of Portland cement, 134-198 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 20-67 parts of heavy calcium powder, 134-217 parts of steel fiber, 23-67 parts of water reducer, and 204-331 parts of water.

[0007] Specifically, in the concrete of the present invention, sulphoaluminate cement, silicate cement, gypsum, silica fume and heavy calcium powder react chemically with water to form needle-shaped crystals such as ettringite and dendrite-shaped fiber crystals, and the addition of quartz sand and bauxite can fill the voids in the concrete, further increase the compactness of the concrete interface, and reduce the shrinkage and expansion rates of the concrete. At the same time, bauxite, as an internal curing agent, can release water in the concrete due to its loose and porous structure to promote the continued hydration of the unhydrated cement matrix, thereby reducing the delayed appearance of ettringite and reducing the cracking of the concrete; and the steel fibers evenly distributed in the concrete further improve the compressive strength, and under the action of silica fume, heavy calcium powder and water reducing agent, the problems of poor fluidity and low workability of the concrete caused by the addition of steel fibers are compensated, thereby improving the practicality of the concrete.

[0008] Preferably, the raw materials for preparation include, by weight:

[0009] 480-500 parts of sulphoaluminate cement, 160-170 parts of Portland cement, 145-165 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 30-50 parts of heavy calcium powder, 150-190 parts of steel fiber, 30-55 parts of water reducer, and 220-300 parts of water.

[0010] It can be understood that the present invention optimizes the raw material ratio of concrete, which can further improve the compressive strength and workability of concrete and achieve the effect of fast hardening and slow setting.

[0011] Preferably, the strength of the sulphoaluminate cement is greater than or equal to 42.5 MPa.

[0012] More preferably, the sulphoaluminate cement is grey low alkalinity fast-hardening sulphoaluminate cement.

[0013] Specifically, the gray low-alkalinity fast-hardening sulphoaluminate cement selected in the present invention not only has the advantages of fast hardening, high strength, low alkalinity and low expansion, but also has the characteristic of low production energy consumption. While achieving fast hardening and high strength of concrete, it also reduces the energy consumption of concrete production, thereby achieving energy conservation and emission reduction.

[0014] Preferably, the strength of the silicate cement is greater than or equal to 52.5 MPa.

[0015] Preferably, the water-to-powder ratio of the gypsum during mixing is 22% to 26%, and the compressive strength of the gypsum after mixing with water and drying is yellow high-strength gypsum of 98 MPa.

[0016] Specifically, yellow high-strength gypsum is a new type of building material. The yellow high-strength gypsum selected in the present invention can promote the hydration reaction of cement, increase the generation of cement gel, make the internal structure of concrete denser, thereby enhancing the strength of concrete and improving the crack resistance of concrete.

[0017] Preferably, the quartz sand is medium sand with a particle size of 0.35 to 0.50 mm and a fineness modulus of 2.5 to 3.0.

[0018] Preferably, the bauxite has a particle size of 1-3 mm and a fineness modulus of 2.5 to 3.0.

[0019] More preferably, the bauxite is calcined bauxite.

[0020] Specifically, the calcined bauxite selected in the present invention has more pores, which can conserve water, keep the interior of the concrete moist, and prevent the concrete from drying out prematurely, thereby reducing the probability of concrete cracking and enhancing the strength of the concrete.

[0021] Preferably, the silica fume contains more than 85% silica by mass;

[0022] The specific gravity of heavy calcium in the heavy calcium powder is greater than or equal to 2.711.

[0023] Preferably, the steel fiber has a length of 10 to 15 mm and a diameter of 0.2 to 0.5 mm.

[0024] More preferably, the steel fiber has a length of 13 mm, a diameter of 0.2 mm, and a tensile strength of 2850 MPa.

[0025] Preferably, the water reducer is a polycarboxylic acid high performance water reducer.

[0026] More preferably, the water reducing agent has a water reducing effect of 40% and an effective solid content of 20% by weight.

[0027] A second aspect of the present invention provides a method for preparing fast-hardening high-strength steel fiber reinforced concrete, comprising the following steps:

[0028] Step 1: Sulphoaluminate cement, silicate cement, gypsum, quartz sand, bauxite, silica fume and heavy calcium powder are mixed and stirred thoroughly to obtain a mixture 1;

[0029] Step 2: fully mix water and a water reducing agent, then add the mixture of water and a water reducing agent into the mixture 1, and stir thoroughly to obtain a mixture 2;

[0030] Step 3: adding the steel fibers evenly into the mixture 2 through a sieve, and stirring thoroughly to obtain fast-hardening high-strength steel fiber reinforced concrete.

[0031] It can be seen from the above technical solutions that the present invention has the following advantages:

[0032] The present invention provides a fast-hardening high-strength steel fiber reinforced concrete, which is prepared from raw materials including, by weight, 450-530 parts of sulphoaluminate cement, 150-180 parts of Portland cement, 134-198 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 20-67 parts of heavy calcium powder, 134-217 parts of steel fiber, 23-67 parts of water reducer, and 204-331 parts of water. The above scheme reduces the risk of concrete cracking, improves the strength of concrete, and reduces the amount of cement used, thereby reducing the production cost of concrete, through the synergistic effect of sulphoaluminate cement, Portland cement, gypsum, quartz sand, bauxite, silica fume, heavy calcium powder, steel fiber, water reducer and water. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0034] Figure 1 The present invention provides a flow chart for preparing a fast-hardening high-strength steel fiber reinforced concrete. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The invention provides a fast-hardening high-strength steel fiber reinforced concrete and a preparation method thereof, which are used to improve the strength of concrete and reduce the cracking risk and production cost of concrete.

[0037] The raw materials and reagents used in the following examples are all commercially available or homemade.

[0038] Example 1

[0039] This embodiment provides a first rapid hardening high strength steel fiber reinforced concrete. The preparation process is shown in Figure 1 , the specific preparation steps are as follows:

[0040] Step 1: according to the mass fractions of each component of Example 1 in Table 1, sulphoaluminate cement, silicate cement, gypsum, quartz sand, bauxite, silica fume and heavy calcium powder are added into a mixer and stirred for 120 seconds to obtain a mixture 1;

[0041] Step 2: Add water and water reducing agent to the mixture 1 of step 1, and continue stirring for 60 seconds to obtain a mixture 2;

[0042] Step 3: Add the steel fiber evenly into the mixture 2 of step 2 through a sieve, and continue stirring for 60 seconds to obtain fast-hardening high-strength steel fiber reinforced concrete.

[0043] Among them, in this embodiment, each group of raw materials needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fiber, a screen needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of concrete. The strength of sulphoaluminate cement is 42.5 MPa or above, the strength of silicate cement is 52.5 MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5-3.0, the fineness modulus of bauxite is 2.5-3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13 mm, a diameter of 0.2 mm and a tensile strength of 2850 MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0044] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0045] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0046] Compared with the rapid-hardening concrete prepared by using an early strength agent, the rapid-hardening high-strength steel fiber reinforced concrete prepared in this embodiment, on the one hand, uses a water-reducing agent to reduce the water-cement ratio, so that the prepared concrete has a longer life, the possibility of concrete cracking will be smaller, and it is less likely to have a honeycombed surface. In addition, without changing the proportions of various raw materials and the strength of concrete, a concrete water-reducing agent of about 0.5% of the mass of mixed cement is used, and the amount of cement is saved by more than 15% to 30%, which greatly reduces the cost of rapid-hardening concrete. On the other hand, the concrete internal curing technology implemented in this embodiment is to add dispersed pre-absorbent materials to the concrete, and the absorbent materials release moisture within a period of time after the concrete solidifies and hardens, so that the hardened concrete is cured, thereby reducing the risk of cracking caused by concrete shrinkage. In the preparation of concrete, a high-strength aggregate with a porous structure, calcined bauxite fine aggregate, is added to replace fine aggregate, which effectively reduces the risk of cracking and improves the mechanical properties of concrete.

[0047] Example 2

[0048] This embodiment provides a second rapid hardening high strength steel fiber reinforced concrete, the preparation steps of which are the same as those of embodiment 1, and the proportions of each component are described in embodiment 2 in reference to table 1.

[0049] Among them, each group of raw materials in this embodiment needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fiber, a sieve needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of concrete; the strength of sulphoaluminate cement is 42.5 MPa or more, the strength of silicate cement is 52.5 MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5 to 3.0, the fineness modulus of bauxite is 2.5 to 3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13 mm, a diameter of 0.2 mm, and a tensile strength of 2850 MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0050] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0051] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0052] Example 3

[0053] This embodiment provides a third type of rapid hardening high-strength steel fiber reinforced concrete, the preparation steps of which are the same as those of embodiment 1, and the proportions of each component are recorded in embodiment 3 in reference to Table 1.

[0054] Among them, each group of raw materials in this embodiment needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fiber, a sieve needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of concrete; the strength of sulphoaluminate cement is 42.5 MPa or more, the strength of silicate cement is 52.5 MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5 to 3.0, the fineness modulus of bauxite is 2.5 to 3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13 mm, a diameter of 0.2 mm, and a tensile strength of 2850 MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0055] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0056] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0057] Example 4

[0058] This embodiment provides a fourth type of rapid hardening high-strength steel fiber reinforced concrete, the preparation steps of which are the same as those of embodiment 1, and the proportions of each component are recorded in embodiment 4 in reference to Table 1.

[0059] Among them, each group of raw materials in this embodiment needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fiber, a sieve needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of concrete; the strength of sulphoaluminate cement is 42.5 MPa or more, the strength of silicate cement is 52.5 MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5 to 3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13 mm, a diameter of 0.2 mm and a tensile strength of 2850 MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0060] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0061] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0062] Example 5

[0063] This embodiment provides a fifth type of rapid hardening high-strength steel fiber reinforced concrete, the preparation steps of which are the same as those of embodiment 1, and the proportions of each component are recorded in embodiment 5 in reference to Table 1.

[0064] Among them, each group of raw materials in this embodiment needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fiber, a sieve needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of concrete; the strength of sulphoaluminate cement is 42.5 MPa or more, the strength of silicate cement is 52.5 MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5 to 3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13 mm, a diameter of 0.2 mm and a tensile strength of 2850 MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0065] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0066] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0067] Example 6

[0068] This embodiment provides a sixth type of rapid hardening high-strength steel fiber reinforced concrete, the preparation steps of which are the same as those of Example 1, and the proportions of each component are recorded in Example 5 in Table 1.

[0069] Among them, each group of raw materials in this embodiment needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding steel fibers, a sieve needs to be used to evenly add the steel fibers to the mixture to prevent them from agglomerating and affecting the fluidity of the concrete.

[0070] Among them, the strength of sulphoaluminate cement is 42.5MPa and above, the strength of silicate cement is 52.5MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5-3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13mm, a diameter of 0.2mm and a tensile strength of 2850MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0071] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0072] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0073] Comparative Example 1

[0074] This comparative example provides a kind of concrete, and its preparation steps are as follows:

[0075] Step 1: according to the mass fractions of the components of Comparative Example 1 in Table 1, sulphoaluminate cement, silicate cement, gypsum, quartz sand, silica fume and heavy calcium powder were added into a mixer and stirred for 120 seconds to obtain a mixture 1;

[0076] Step 2: Add water and water reducing agent to the mixture 1 of step 1, and continue stirring for 60 seconds to obtain a mixture 2;

[0077] Step 3: Evenly add the steel fiber to the mixture 2 in step 2 through a sieve, and continue stirring for 60 seconds to obtain concrete. In this embodiment, each group of raw materials needs to be stirred evenly, and the particle size of quartz sand and bauxite needs to be controlled between 1 and 3 mm. When adding the steel fiber, a sieve needs to be used to evenly add the steel fiber to the mixture to prevent it from agglomerating and affecting the fluidity of the concrete.

[0078] Among them, the strength of sulphoaluminate cement is 42.5MPa and above, the strength of silicate cement is 52.5MPa, the water-powder ratio of gypsum is 24%, the fineness modulus of quartz sand is 2.5-3.0, the steel fiber is a copper-plated straight steel fiber with a length of 13mm, a diameter of 0.2mm and a tensile strength of 2850MPa, and the water reducer is a polycarboxylic acid high-performance water reducer.

[0079] The concrete of this embodiment is naturally cured for 7 days. During the natural curing period, the concrete needs to be watered and cured to make the surface of the concrete specimen completely wet, and the water needs to be poured three times a day. After the natural curing is completed, conventional curing is performed for 21 days, and the concrete is cured for a total of 28 days. During this period, the 4h compressive strength, 7d compressive strength, 28-day compressive strength, slump, initial setting time and final setting time of the concrete of this embodiment are tested respectively, and a total of 6 data are obtained. The test results are shown in Table 2.

[0080] After 28 days of concrete curing, the concrete specimens were subjected to a temperature cycle experiment. The temperature was raised for 4 hours and lowered for 3 hours to simulate the temperature cycle of concrete under sunlight. The number of experimental cycles was 100. The target temperature of each heating was 75°C, and the target temperature of each cooling should reach 25°C. After the temperature cycle experiment, the concrete was subjected to a compressive strength test. The test results are shown in Table 2.

[0081] Table 1. Ratios of raw materials for preparation of Examples 1 to 6 and Comparative Example 1

[0082]

[0083] Note: The data of each component in Table 1 represent the mass fraction of each component.

[0084] Table 2. Test results of Examples 1 to 6 and Comparative Example 1

[0085]

[0086] Note: The original height of the concrete specimens prepared in Examples 1 to 6 and Comparative Example 1 was 30.2 cm.

[0087] According to the test results of the present invention,

[0088] In Examples 1 to 3, the ratio of quartz sand and bauxite is adjusted, and the amount of bauxite used is 200 to 650 parts, which can achieve good compressive strength, among which Example 2 has the best effect. In addition, quartz sand is 2.5 yuan per kilogram, and bauxite is about 1.2 yuan per kilogram. The present invention reduces the cost by adding a large amount of bauxite material and reducing the amount of quartz sand and cement without reducing the strength of concrete as much as possible, so that the cost of the present invention is reduced.

[0089] The amount of water reducer used in Examples 4 to 6 is adjusted according to the amount of water reducer used in Examples 1 to 3. The amount of water reducer used in Examples 4 to 5 is less than that used in Examples 1 to 2. This is because the use of water reducer can increase the fluidity of concrete, but it weakens the strength of such concrete. Therefore, the concrete strength of Examples 4 to 5 is stronger. However, adding too little water reducer will lead to poor fluidity, which is not conducive to the actual construction of the project. In Example 6, adding too much water reducer reduces the strength of the concrete. When the components of Examples 1 to 3 are selected, that is, 55 parts of water reducer are used, both strength and fluidity requirements can be met at the same time.

[0090] In Comparative Example 1, no bauxite was added, and the strength of the obtained concrete was significantly lower than that of the embodiment.

[0091] It can be seen from the experimental data that the various properties of the embodiments of the present invention are better than those of the comparative examples. The highest compressive strength of the embodiments reaches 83.6MPa, and the maximum slump is 251mm. This shows that the present invention utilizes the bridging effect of steel fibers, the slow setting of gypsum and the high temperature resistance and internal curing technology of bauxite, combined with the composite cementitious material system of sulfate cement, silicate cement, quartz sand, silica fume, and heavy calcium powder, to develop high-strength fast-hardening steel fiber reinforced concrete, solving the problems of low long-term strength, low durability and easy cracking of traditional fast-hardening concrete. The high-strength fast-hardening steel fiber reinforced concrete prepared by the technical method of the present invention has strong workability, large slump, extremely high early strength of the concrete and high long-term strength, and the 4h compressive strength can reach more than 30MPa, the 7d compressive strength can reach more than 54.2MPa, and the 28d compressive strength can reach more than 72.5MPa; the concrete has the characteristics of temperature resistance, and can still maintain high strength under multiple day and night temperature changes, and by using bauxite, the use of quartz sand is reduced, and the cement dosage is less than 710kg / m 3 , thereby reducing the preparation cost of concrete. In addition, the concrete curing conditions in the present invention are simple and ordinary curing conditions can be used.

[0092] It should be noted that the present invention uses concrete with a larger slump, which means that it has better fluidity and workability, is more in line with the requirements of the construction site, and can be more conveniently poured.

[0093] In summary, the solution of the present invention has the following beneficial effects:

[0094] (1) The present invention adopts optimized cementitious materials and their proportions, and utilizes the hydration reaction of gypsum and sulphoaluminate cement to achieve the effect of fast hardening and slow setting, thereby avoiding cracking of concrete due to violent hydration reaction and meeting the actual time requirements of emergency repair projects.

[0095] (ii) The present invention utilizes the internal curing mechanism of bauxite to reduce the probability of concrete cracking. At the same time, the average elastic modulus of bauxite is 207 GPa, and it has a high compressive strength. The addition of bauxite can increase the compressive strength of concrete by nearly 20%.

[0096] (III) The present invention reduces the cost by adding materials such as silica fume and bauxite to reduce the amount of quartz sand and cement used without reducing the strength of concrete as much as possible, thereby reducing the cost of the present invention.

[0097] (iv) The present invention utilizes the bridging effect and high tensile strength of copper-plated straight steel fibers with a tensile strength of 2850 MPa, and evenly distributes the steel fibers inside the concrete through a screen, thereby further improving the compressive strength of the concrete.

[0098] (V) The present invention utilizes the mechanism that polycarboxylate water reducer can form a layer of water film on the surface of cement and aggregate to reduce the sliding resistance between particles, thereby making the interior of the concrete uniform and dense, avoiding the problem of uneven and non-dense internal structure of the concrete after using the early strength agent.

[0099] (VI) The rapid hardening steel fiber reinforced concrete of the present invention can be used in a variety of fields such as bridge expansion joints, bridge deck paving, and emergency repair projects, and has the characteristics of wide application and easy construction.

[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A fast-hardening high-strength steel fiber reinforced concrete, It is characterized in that The raw materials for preparation include, by weight: 450-530 parts of sulphoaluminate cement, 150-180 parts of silicate cement, 134-198 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 20-67 parts of heavy calcium powder, 134-217 parts of steel fiber, 23-67 parts of water reducer, and 204-331 parts of water; The strength of the sulphoaluminate cement is greater than or equal to 42.5 MPa; The strength of the silicate cement is greater than or equal to 52.5 MPa; The quartz sand has a particle size of 0.35 to 0.50 mm and a fineness modulus of 2.5 to 3.0; The bauxite has a particle size of 1 to 3 mm and a fineness modulus of 2.5 to 3.0; The mass content of silicon dioxide in the silicon ash is above 85%; The specific gravity of heavy calcium in the heavy calcium powder is greater than or equal to 2.

711.

2. The rapid hardening high strength steel fiber reinforced concrete according to claim 1, It is characterized in that The raw materials for preparation include, by weight: 480-500 parts of sulphoaluminate cement, 160-170 parts of Portland cement, 145-165 parts of gypsum, 400-1025 parts of quartz sand, 200-650 parts of bauxite, 187-240 parts of silica fume, 30-50 parts of heavy calcium powder, 150-190 parts of steel fiber, 30-55 parts of water reducer, and 220-300 parts of water.

3. The rapid hardening high strength steel fiber reinforced concrete according to claim 1, It is characterized in that The steel fiber has a length of 10 to 15 mm and a diameter of 0.2 to 0.5 mm.

4. The rapid hardening high strength steel fiber reinforced concrete according to claim 1, It is characterized in that The water reducing agent is a polycarboxylic acid high performance water reducing agent.

5. A method for preparing the rapid hardening high-strength steel fiber reinforced concrete according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Step 1: Sulphoaluminate cement, silicate cement, gypsum, quartz sand, bauxite, silica fume and heavy calcium powder are mixed and stirred thoroughly to obtain a mixture 1; Step 2: fully mix water and a water reducing agent, then add the mixture of water and a water reducing agent into the mixture 1, and stir thoroughly to obtain a mixture 2; Step 3: adding the steel fibers evenly into the mixture 2 through a sieve, and stirring thoroughly to obtain fast-hardening high-strength steel fiber reinforced concrete.