Preparation method and application of carbon nitride-based catalyst for inhibiting photogenerated carrier recombination

The CoOOH/CN composite catalyst was prepared through loading and morphology modulation technology, which solved the problems of small specific surface area and high photogenerated electron recombination rate of carbon nitride-based catalysts, achieved efficient PMS activation and organic pollutant degradation, and improved the performance of the catalyst. Photocurrent response performance and removal rate of sulfonamide antibiotics.

CN117920298BActive Publication Date: 2024-10-11NANJING INST OF ENVIRONMENTAL SCI MINIST OF ECOLOGY & ENVIRONMENT OF THE PEOPLES REPUBLIC OF CHINA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311698511.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2024-10-11
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

Carbon nitride-based catalysts have small specific surface area, low visible light utilization rate, and fast complexation speed of photogenerated electron pairs, which limits their application in PMS activation and organic pollutant degradation.

Method used

The CoOOH/CN composite catalyst was prepared through loading and morphology modulation methods, using carbon fiber as a hard template to increase the specific surface area and active sites of g-C3N4 fiber, reduce the photogenerated electron-hole recombination rate, and accelerate the activation of PMS.

Benefits of technology

The photocurrent response performance and catalytic efficiency of the catalyst are significantly improved, the degradation ability of sulfonamide antibiotics is enhanced, and the leaching pollution of cobalt ions is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920298B_ABST
    Figure CN117920298B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photocatalyst preparation, and in particular to a preparation method and application of a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination. The preparation method comprises the following steps: preparing carbon nanofibers, preparing carboxylated carbon nanofibers, directional arranging carboxylated carbon nanofibers, preparing carbon nitride fibers, and preparing a CoOOH / CN composite catalyst. The preparation method designed by the invention obtains a CoOOH / CN composite catalyst by composite CoOOH with g-C3N4 fibers with a high specific surface area. In the process of activating peroxymonosulfate to degrade organic pollutant antibiotics, the problem that single nano CoOOH is prone to agglomeration and catalytic active sites are reduced, thereby reducing catalytic efficiency can be effectively solved. Furthermore, the g-C3N4 fibers, as electron donors, can effectively promote the valence state conversion of cobalt ions in CoOOH in the process of activating peroxymonosulfate, thereby enhancing the catalytic efficiency and reducing the leaching pollution of cobalt ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalyst preparation, and in particular to a preparation method and application of a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination. Background Art

[0002] For a long time, the extensive use of sulfonamide antibiotics has had adverse effects on the ecosystem because their chemical structure is stable and not easily degraded. Traditional wastewater treatment technology is not ideal for the removal of sulfonamide antibiotics. Photocatalytic technology based on semiconductor materials has the advantages of mild reaction conditions, low cost, and environmental friendliness, and shows great potential in degrading sulfonamide antibiotics.

[0003] Peroxymonosulfate (PMS) activation based on advanced oxidation processes has unique advantages in removing organic pollutants. It degrades pollutants in water by producing ·SO4 free radicals to oxidize them. Compared with ·OH, ·SO4 has higher oxidation capacity and longer survival time, and has sufficient time and ability to degrade and remove various pollutants in water.

[0004] As a common photocatalyst, graphene nitride (CN) has attracted much attention due to its stable chemical properties and convenient preparation. However, due to its small specific surface area, low visible light utilization rate, and fast complexation rate of photogenerated electron pairs, it has little effect on the active activation of PMS under visible light irradiation, which seriously limits its wide application.

[0005] Therefore, the present invention modifies CN by means of loading and morphology modulation, thereby improving its activation effect on PMS and synergistically oxidizing and degrading organic pollutants. Summary of the invention

[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a carbon nitride-based catalyst for inhibiting the recombination of photogenerated carriers, as shown below.

[0007] S1. Preparation of carbon nanofibers:

[0008] Carbon nanofibers, denoted as CNF, were prepared by combining dynamic crystallization and high-temperature calcination;

[0009] S2. Preparation of carboxylated carbon nanofibers:

[0010] The CNF prepared in S1 was mixed with mixed acid, and then subjected to ultrasonic stirring, filtration, washing, and drying to obtain carboxylated carbon nanofibers, which were denoted as CNF-COOH;

[0011] S3, oriented carboxylated carbon nanofibers:

[0012] First, the CNF-COOH prepared in S2 is mixed and dispersed in DMF to obtain a mixed solution with a concentration of 10 to 12 g / L, and then the mixed solution is added to a reactor with parallel electrodes at the bottom, and an electric field is applied;

[0013] S4, preparing nitrided carbon fibers:

[0014] S4-1, firstly add dicyandiamide to the reactor in S3, heat it under a first temperature gradient under oscillation conditions, turn off the electric field after the reaction is completed, and finally volatilize the solvent and dry it to obtain a solid powder; the mass ratio of dicyandiamide to CNF-COOH is 4 to 6:1;

[0015] S4-2, placing the solid powder prepared in S4-1 into a mixed atmosphere, and heating it under a second temperature gradient to obtain carbon self-doped carbon nitride fiber, which is recorded as g-C3N4 fiber;

[0016] S5. Preparation of CoOOH / CN composite catalyst:

[0017] First, add Co(NO3)2·6H2O solution to a reactor with parallel electrodes at the bottom; then add g-C3N4 fiber prepared by S4-2 and apply electric field, and ultrasonically treat for 25-35 minutes; then add NaOH solution and react at 45-50°C for 2-3 minutes; then add H2O2 and react at 45-55°C for 4.5-6 hours before turning off the electric field; finally, wash and dry the precipitate obtained after the reaction to obtain a composite fiber in which CoOOH is loaded on g-C3N4 fiber, i.e., CoOOH / CN composite catalyst;

[0018] Let n be the multiplication number and n∈R + When the amount of g-C3N4 fiber added is n·1g, the amount of Co(NO3)2·6H2O solution added with a mass fraction of 20% is n·[40,60]mL, the amount of NaOH solution added with a mass fraction of 4% is n·[6,10]mL, and the amount of H2O2 added with a mass fraction of 30% is n·[4,8]mL.

[0019] Further, in S4-1: the first temperature gradient is: first, uniformly increase the temperature from room temperature to 40°C within 3 to 5 minutes, and keep it warm for 1 to 2 minutes; then, uniformly increase the temperature from 40°C to 60°C within 3 to 5 minutes, and keep it warm for 2 to 3 minutes; then, uniformly increase the temperature from 60°C to 90°C within 1 to 2 minutes, and keep it warm for 9 to 10 hours; finally, naturally cool to room temperature;

[0020] The temperature at which the solvent evaporates is 55-65°C;

[0021] In S4-2: the volume ratio of nitrogen to air in the mixed atmosphere is 4 to 4.5:1;

[0022] The second temperature gradient is: first, uniformly increase the temperature from room temperature to 50°C within 6 to 8 minutes, and keep it warm for 4 to 5 minutes; then, uniformly increase the temperature from 80°C to 100°C within 2 to 3 minutes, and keep it warm for 3 to 5 minutes; then, uniformly increase the temperature from 100°C to 300°C within 15 to 20 minutes, and keep it warm for 9 to 10 minutes; then, uniformly increase the temperature from 300°C to 500°C within 15 to 20 minutes, and keep it warm for 2 to 3 hours; finally, naturally cool to room temperature.

[0023] Description: The present invention uses carbon fiber as a hard template to prepare fibrous cobalt-loaded g-C3N4 fibers, and gradually removes the hard template in the subsequent gradient heating process to obtain g-C3N4 fibers with high specific surface area and active sites. In the above process, the carbon remaining after pyrolysis can act as an acceptor of photogenerated electrons, reduce the recombination rate of photogenerated electrons-holes, and accelerate the activation of PMS.

[0024] Furthermore, the method for preparing carbon nanofibers in S1 is:

[0025] S1-1. First, add trimesic acid, zinc acetate dihydrate and DMF into a reactor and stir evenly for 30 to 40 minutes to obtain a mixed solution; the concentration of trimesic acid in the mixed solution is 0.06 to 0.065 mmol / L, and the concentration of zinc acetate dihydrate is 0.18 to 0.20 mmol / L;

[0026] S1-2, then the mixed solution in S1-1 is dynamically crystallized at 90-100°C for 3-3.5h, and after the dynamic crystallization is completed, it is naturally cooled to room temperature to obtain a zinc-trimethylenetetracarboxylic acid metal organic framework, and the zinc-trimethylenetetracarboxylic acid metal organic framework is washed with DMF and then vacuum dried at 75-85°C for 10-12h;

[0027] S1-3, finally, the solid powder after vacuum drying in S1-2 is subjected to high temperature treatment under a third temperature gradient to obtain carbon nanofibers, which are recorded as CNF;

[0028] The third temperature gradient is: first, the temperature is uniformly increased from room temperature to 100°C within 8 to 10 minutes, and kept warm for 4 to 5 minutes; then, the temperature is uniformly increased from 100°C to 300°C within 8 to 10 minutes, and kept warm for 3 to 5 minutes; then, the temperature is uniformly increased from 300°C to 600°C within 10 to 15 minutes, and kept warm for 1 to 1.5 minutes; secondly, the temperature is uniformly increased from 600°C to 950°C within 10 to 15 minutes, and kept warm for 2 to 3 hours; finally, it is naturally cooled to room temperature.

[0029] Description: The above method can be used to obtain high-quality and high-yield g-C3N4 fibers through dynamic crystallization at a lower temperature. The specific surface area of ​​the obtained g-C3N4 fibers is greatly increased compared with CN sheets, which enhances the separation and transfer of photogenerated charges. Moreover, the carbon fibers as hard templates can be removed by pyrolysis, and a small amount of residue will not reduce the performance of the g-C3N4 fibers. Moreover, the residual carbon after pyrolysis can act as an acceptor for photogenerated electrons, reduce the recombination rate of photogenerated electrons and holes, and accelerate the activation of PMS.

[0030] Furthermore, the method for preparing carboxylated carbon nanofibers in S2 is:

[0031] S2-1, mixing concentrated sulfuric acid and concentrated nitric acid to prepare a mixed acid;

[0032] S2-2, adding CNF and mixed acid prepared in S1 into the reactor successively, and ultrasonically treating at 40-50 kHz for 30-35 min;

[0033] Let n be the multiplication number and n∈R + , when the amount of CNF added is n·1g, the amount of concentrated sulfuric acid with a mass fraction of 98% added is n[30,33]mL, and the amount of concentrated nitric acid with a mass fraction of 65% added is n[10,11]mL.

[0034] S2-3, the product after ultrasonic treatment in S2-2 was stirred in a water bath at 80-90°C for 60-70 minutes, and naturally cooled to room temperature after the reaction;

[0035] S2-4, dilute the product treated in S2-3 5 times with pure water, filter it with a microporous filter membrane with a pore size of 0.22 μm, and then wash and filter it repeatedly until the washed product is neutral;

[0036] S2-5. The product washed to neutrality in S2-4 was dried under vacuum at 80° C. for 24 h to obtain carboxylated carbon nanofibers, which were recorded as CNF-COOH.

[0037] Description: Unfunctionalized carbon nanofibers have a small diameter, large surface energy, and strong van der Waals forces between them, so they are very easy to agglomerate. They are difficult to disperse or dissolve in organic and inorganic solvents. After the carbon nanofibers are treated with mixed acid, the particles are reduced, the ports are opened, and carboxyl functional groups are introduced, the entanglement and agglomeration are reduced, and the dispersibility and stability in the solution are significantly improved.

[0038] Furthermore, the gap between the parallel electrodes in S3 is 3-5 μm, the voltage amplitude of the AC voltage applied to the parallel electrodes is 10-15 V, and the frequency is 4-5 MHz.

[0039] Description: When a drop of carbon nanofiber suspension is added to parallel microelectrodes with an alternating electric field, the carbon nanofibers will be polarized under the action of the external electric field due to their dielectric properties. Since the spatial distribution of the external electric field is uneven, these polarized carbon nanofibers will move to the high electric field area under the action of the external electric field force. Therefore, we can use parallel electrodes to make the carbon nanofibers deposit in a directional manner between the electrodes to avoid entanglement and agglomeration.

[0040] Compared with the existing preparation method of CN catalyst, the beneficial effects of the present invention are:

[0041] (1) The CoOOH / CN composite catalyst designed by the present invention is obtained by compounding CoOOH on g-C3N4 fiber with a high specific surface area. In the process of activating peroxymonosulfate to degrade organic pollutant antibiotics, the problem that single nano-CoOOH is prone to agglomeration, the catalytic active sites are reduced, and the catalytic efficiency is reduced; and the g-C3N4 fiber as an electron donor can effectively promote the valence state conversion of cobalt ions in CoOOH during the photoactivated PMS process, thereby enhancing the catalytic efficiency and reducing the leaching pollution of cobalt ions.

[0042] (2) In the CoOOH / CN composite catalyst designed by the present invention, the loading of CoOOH significantly inhibits the recombination of photogenerated carriers; therefore, CoOOH / CN exhibits good photocurrent response performance, that is, its photogenerated electron-hole separation efficiency is higher, which can enhance the catalytic efficiency of photoactivated PMS.

[0043] (3) When preparing the matrix of the CoOOH / CN composite catalyst, the present invention uses an external electric field to make the g-C3N4 fibers oriented and deposited in parallel between the electrodes. Therefore, in the subsequent preparation process, the entanglement and agglomeration of the fibers can be effectively avoided, so that the prepared CoOOH / CN composite catalyst has a larger specific surface area and more active sites. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is a flow chart of the preparation method of the present invention;

[0045] Figure 2 (a) is the HRTEM image and (d) Mapping image of the CoOOH / CN composite catalyst in the experimental example, where a, b, c are HRTEM images at 200nm, 10nm and 5nm, respectively, and d is the Mapping image. DETAILED DESCRIPTION

[0046] In order to further explain the method and effect of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings.

[0047] Example 1

[0048] Example 1 mainly describes the design of the present invention under specific parameters.

[0049] S1. Preparation of carbon nanofibers:

[0050] Carbon nanofibers, denoted as CNF, were prepared by combining dynamic crystallization and high-temperature calcination;

[0051] S1-1. First, add trimesic acid, zinc acetate dihydrate and DMF into a reactor and stir evenly for 30 minutes to obtain a mixed solution; the concentration of trimesic acid in the mixed solution is 0.06 mmol / L, and the concentration of zinc acetate dihydrate is 0.18 mmol / L;

[0052] S1-2, then the mixed solution in S1-1 was subjected to dynamic crystallization at 90°C for 3 hours, and after the dynamic crystallization was completed, it was naturally cooled to 20°C to obtain a zinc-trimethylenetetracarboxylic acid metal organic framework, and the zinc-trimethylenetetracarboxylic acid metal organic framework was washed with DMF and vacuum dried at 75°C for 10 hours;

[0053] S1-3, finally, the solid powder after vacuum drying in S1-2 is subjected to high temperature treatment under a third temperature gradient to obtain carbon nanofibers, which are recorded as CNF;

[0054] The third temperature gradient is: first, uniformly increase the temperature from 20°C to 100°C within 8 minutes, and keep it warm for 4 minutes; then, uniformly increase the temperature from 100°C to 300°C within 8 minutes, and keep it warm for 3 minutes; then, uniformly increase the temperature from 300°C to 600°C within 10 minutes, and keep it warm for 1 minute; then, uniformly increase the temperature from 600°C to 950°C within 10 minutes, and keep it warm for 2 hours; finally, naturally cool to 20°C;

[0055] S2. Preparation of carboxylated carbon nanofibers:

[0056] The CNF prepared in S1 was mixed with mixed acid, and then subjected to ultrasonic stirring, filtration, washing, and drying to obtain carboxylated carbon nanofibers, which were denoted as CNF-COOH.

[0057] S2-1, mixing concentrated sulfuric acid and concentrated nitric acid to prepare a mixed acid;

[0058] S2-2, adding CNF and mixed acid prepared in S1 into the reactor successively, and ultrasonically treating at 40 kHz for 30 min;

[0059] The amount of CNF added was 1 g, the amount of 98% concentrated sulfuric acid added was 30 mL, and the amount of 65% concentrated nitric acid added was 10 mL;

[0060] S2-3, the product after ultrasonic treatment of S2-2 was stirred in a water bath at 80°C for 60 min, and naturally cooled to 20°C after the reaction;

[0061] S2-4, dilute the product treated in S2-3 5 times with pure water, filter it with a microporous filter membrane with a pore size of 0.22 μm, and then wash and filter it repeatedly until the washed product is neutral;

[0062] S2-5, drying the neutralized product in S2-4 under vacuum at 80°C for 24 h to obtain carboxylated carbon nanofibers, denoted as CNF-COOH;

[0063] S3, oriented carboxylated carbon nanofibers:

[0064] First, the CNF-COOH prepared in S2 was mixed and dispersed in DMF to obtain a mixed solution with a concentration of 10 g / L, and then the mixed solution was added to a reactor with parallel electrodes at the bottom and an electric field was applied;

[0065] The gap between the parallel electrodes is 3 μm, and the voltage amplitude of the AC voltage on the parallel electrodes is 10 V and the frequency is 4 MHz;

[0066] S4, preparing nitrided carbon fibers:

[0067] S4-1, firstly add dicyandiamide to the reactor in S3, heat it under a first temperature gradient under oscillation conditions, turn off the electric field after the reaction is completed, and finally volatilize the solvent and dry it to obtain a solid powder; the mass ratio of dicyandiamide to CNF-COOH is 4:1;

[0068] The first temperature gradient is: first, uniformly increase the temperature from 20°C to 40°C within 3 minutes and keep it warm for 1 minute; then, uniformly increase the temperature from 40°C to 60°C within 3 minutes and keep it warm for 2 minutes; then, uniformly increase the temperature from 60°C to 90°C within 1 minute and keep it warm for 9 hours; finally, naturally cool to 20°C;

[0069] The temperature at which the solvent evaporates is 55°C;

[0070] S4-2, placing the solid powder prepared in S4-1 into a mixed atmosphere, and heating it under a second temperature gradient to obtain carbon-loaded nitride carbon fibers, which are recorded as g-C3N4 fibers;

[0071] In S4-2: the volume ratio of nitrogen to air in the mixed atmosphere is 4:1;

[0072] The second temperature gradient is: first, uniformly increase the temperature from 20°C to 50°C within 6 minutes, and keep it warm for 4 minutes; then, uniformly increase the temperature from 80°C to 100°C within 2 minutes, and keep it warm for 3 minutes; then, uniformly increase the temperature from 100°C to 300°C within 15 minutes, and keep it warm for 9 minutes; then, uniformly increase the temperature from 300°C to 500°C within 15 minutes, and keep it warm for 2 hours; finally, naturally cool to 20°C;

[0073] S5. Preparation of CoOOH / CN composite catalyst:

[0074] First, add Co(NO3)2·6H2O solution to a reactor with parallel electrodes at the bottom; then add g-C3N4 fiber prepared by S4-2 and apply electric field, and ultrasonic treatment for 25 minutes; then add NaOH solution and react at 45℃ for 2 minutes; then add H2O2 and react at 45℃ for 4.5 hours before turning off the electric field; finally, wash and dry the precipitate obtained after the reaction to obtain a composite fiber loaded with CoOOH on g-C3N4 fiber, i.e., CoOOH / CN composite catalyst;

[0075] The added amount of g-C3N4 fiber was 1 g, the added amount of 20% Co(NO3)2·6H2O solution was 50 mL, the added amount of 4% NaOH solution was 8 mL, and the added amount of 30% H2O2 was 6 mL.

[0076] Example 2

[0077] The description of Example 2 is based on the scheme described in Example 1, and is intended to illustrate the scheme design under another parameter.

[0078] S1. Preparation of carbon nanofibers:

[0079] Carbon nanofibers, denoted as CNF, were prepared by combining dynamic crystallization and high-temperature calcination;

[0080] S1-1. First, add trimesic acid, zinc acetate dihydrate and DMF into a reactor and stir evenly for 40 minutes to obtain a mixed solution; the concentration of trimesic acid in the mixed solution is 0.065 mmol / L, and the concentration of zinc acetate dihydrate is 0.20 mmol / L;

[0081] S1-2, then the mixed solution in S1-1 was subjected to dynamic crystallization at 100°C for 3.5 hours, and after the dynamic crystallization was completed, it was naturally cooled to 20°C to obtain a zinc-trimethylenetetracarboxylic acid metal organic framework, and the zinc-trimethylenetetracarboxylic acid metal organic framework was washed with DMF and then vacuum dried at 85°C for 12 hours;

[0082] S1-3, finally, the solid powder after vacuum drying in S1-2 is subjected to high temperature treatment under a third temperature gradient to obtain carbon nanofibers, which are recorded as CNF;

[0083] The third temperature gradient is: first, uniformly increase the temperature from 20°C to 100°C within 10 minutes, and keep it warm for 5 minutes; then, uniformly increase the temperature from 100°C to 300°C within 10 minutes, and keep it warm for 5 minutes; then, uniformly increase the temperature from 300°C to 600°C within 15 minutes, and keep it warm for 1.5 minutes; then, uniformly increase the temperature from 600°C to 950°C within 15 minutes, and keep it warm for 3 hours; finally, naturally cool to 20°C;

[0084] S2. Preparation of carboxylated carbon nanofibers:

[0085] The CNF prepared in S1 was mixed with mixed acid, and then subjected to ultrasonic stirring, filtration, washing, and drying to obtain carboxylated carbon nanofibers, which were denoted as CNF-COOH.

[0086] S2-1, mixing concentrated sulfuric acid and concentrated nitric acid to prepare a mixed acid;

[0087] S2-2, adding CNF and mixed acid prepared in S1 into the reactor successively, and ultrasonically treating at 50 kHz for 35 min;

[0088] The amount of CNF added was 1 g, the amount of 98% concentrated sulfuric acid added was 33 mL, and the amount of 65% concentrated nitric acid added was 11 mL;

[0089] S2-3, the product after ultrasonic treatment of S2-2 was stirred in a water bath at 90°C for 70 minutes, and naturally cooled to 20°C after the reaction;

[0090] S2-4, dilute the product treated in S2-3 5 times with pure water, filter it with a microporous filter membrane with a pore size of 0.22 μm, and then wash and filter it repeatedly until the washed product is neutral;

[0091] S2-5, drying the neutralized product in S2-4 under vacuum at 80°C for 24 h to obtain carboxylated carbon nanofibers, denoted as CNF-COOH;

[0092] S3, oriented carboxylated carbon nanofibers:

[0093] First, the CNF-COOH prepared in S2 was mixed and dispersed in DMF to obtain a mixed solution with a concentration of 12 g / L. The mixed solution was then added to a reactor with parallel electrodes at the bottom and an electric field was applied.

[0094] The gap between the parallel electrodes is 5 μm, and the voltage amplitude of the AC voltage on the parallel electrodes is 15 V and the frequency is 5 MHz;

[0095] S4, preparing nitrided carbon fibers:

[0096] S4-1, firstly add dicyandiamide to the reactor in S3, heat it under a first temperature gradient under oscillation conditions, turn off the electric field after the reaction is completed, and finally volatilize the solvent and dry it to obtain a solid powder; the mass ratio of dicyandiamide to CNF-COOH is 6:1;

[0097] The first temperature gradient is: first, uniformly increase the temperature from 20°C to 40°C within 5 minutes and keep it warm for 2 minutes; then, uniformly increase the temperature from 40°C to 60°C within 5 minutes and keep it warm for 3 minutes; then, uniformly increase the temperature from 60°C to 90°C within 2 minutes and keep it warm for 10 hours; finally, naturally cool to 20°C;

[0098] The temperature at which the solvent evaporates is 65°C;

[0099] S4-2, placing the solid powder prepared in S4-1 into a mixed atmosphere, and heating it under a second temperature gradient to obtain carbon-loaded nitride carbon fibers, which are recorded as g-C3N4 fibers;

[0100] In S4-2: the volume ratio of nitrogen to air in the mixed atmosphere is 4.5:1;

[0101] The second temperature gradient is: first, uniformly increase the temperature from 20°C to 50°C within 8 minutes, and keep it warm for 5 minutes; then, uniformly increase the temperature from 80°C to 100°C within 3 minutes, and keep it warm for 5 minutes; then, uniformly increase the temperature from 100°C to 300°C within 20 minutes, and keep it warm for 10 minutes; then, uniformly increase the temperature from 300°C to 500°C within 20 minutes, and keep it warm for 3 hours; finally, naturally cool to 20°C;

[0102] S5. Preparation of CoOOH / CN composite catalyst:

[0103] First, add Co(NO3)2·6H2O solution to a reactor with parallel electrodes at the bottom; then add g-C3N4 fiber prepared by S4-2 and apply electric field, and ultrasonic treatment for 35 minutes; then add NaOH solution and react at 50℃ for 3 minutes; then add H2O2 and react at 55℃ for 6 hours before turning off the electric field; finally, wash and dry the precipitate obtained after the reaction to obtain a composite fiber loaded with CoOOH on g-C3N4 fiber, i.e., CoOOH / CN composite catalyst;

[0104] The added amount of g-C3N4 fiber was 1 g, the added amount of 20% Co(NO3)2·6H2O solution was 80 mL, the added amount of 4% NaOH solution was 10 mL, and the added amount of 30% H2O2 was 6 mL.

[0105] Experimental example

[0106] The description of this experimental example is based on the description scheme in Example 2, and is intended to illustrate the practical application effect of the present invention.

[0107] 1. Experimental design

[0108] A certain amount of CoOOH / CN composite catalyst was dispersed in pure water, the concentration of the pollutant sulfamethoxazole was 20ppm, and PMS was 50mM; a 500W xenon lamp was used with a 420nm filter to simulate visible light.

[0109] First, stir the mixed solution in a dark environment for 30 minutes. After the solution reaches adsorption equilibrium, turn on the light to enter the light reaction stage, and then turn on the light for photocatalytic degradation reaction. Sampling is performed at regular intervals. The samples are filtered with a 0.22m filter head and the pollutant concentration is tested.

[0110] 2. Related performance experiments

[0111] To compare the actual performance of the present invention under different experimental conditions, the following experimental groups were designed:

[0112] Control group 1: The catalyst was pure CN fiber;

[0113] Control group 2: The catalyst is pure CoOOH;

[0114] Experimental group 1: the catalyst is: CoOOH / CN composite catalyst with a CoOOH loading of 3%, recorded as 3% CoOOH / CN;

[0115] Experimental group 2: The catalyst is: CoOOH / CN composite catalyst with a CoOOH loading of 5%, recorded as 5% CoOOH / CN;

[0116] Experimental group 3: The catalyst is: CoOOH / CN composite catalyst with a CoOOH loading of 10%, recorded as 10% CoOOH / CN;

[0117] Experimental group 4: the catalyst is: CoOOH / CN composite catalyst with a CoOOH loading of 15%, recorded as 15% CoOOH / CN;

[0118] Experimental Group 5: The catalyst is: CoOOH / CN composite catalyst with a CoOOH loading of 20%, recorded as 20% CoOOH / CN.

[0119] The experimental results are shown in Table 1.

[0120] Table 1 Percentage of residual pollutants at different reaction times

[0121]

[0122]

[0123] It can be seen from the data in Table 1 that the CoOOH / CN composite catalyst prepared by the present invention has a better synergistic effect with PMS than the simple CN fiber catalyst or CoOOH catalyst, and has the highest degradation rate for the pollutant sulfamethoxazole, which can reach a removal rate of nearly 70% to 80% when the reaction time is 100 minutes.

[0124] It is worth noting that, in the same reaction time, when the CoOOH loading is gradually increased from 3% to 20%, the catalytic efficiency of the CoOOH / CN composite catalyst to enhance the photoactivated peroxymonosulfate shows a trend of first increasing and then decreasing; this is because the excess CoOOH is not evenly loaded on the CN fiber, and the excess part blocks the micropores and active sites, causing the photoelectric performance of the catalyst to decrease. In this embodiment, the CoOOH / CN composite catalyst with a CoOOH loading of 10% exhibits the best catalytic performance.

[0125] The reason for the above phenomenon is that the loading of CoOOH significantly inhibits the recombination of photogenerated carriers; therefore, CoOOH / CN exhibits a higher photocurrent response than pure CN. Therefore, the photogenerated electron-hole separation efficiency in the CoOOH / CN catalyst is higher, which can enhance the catalytic efficiency of photoactivated peroxymonosulfate.

Claims

1. A method for preparing a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination, characterized in that: The following steps are involved: S1. Preparation of carbon nanofibers: Carbon nanofibers, denoted as CNF, were prepared by combining dynamic crystallization and high-temperature calcination; S2. Preparation of carboxylated carbon nanofibers: The CNF prepared in S1 was mixed with mixed acid, and then subjected to ultrasonic stirring, filtration, washing, and drying to obtain carboxylated carbon nanofibers, which were denoted as CNF-COOH; S3, oriented carboxylated carbon nanofibers: First, the CNF-COOH prepared in S2 is mixed and dispersed in DMF to obtain a mixed solution with a concentration of 10 to 12 g / L, and then the mixed solution is added to a reactor with parallel electrodes at the bottom, and an electric field is applied; S4, preparing carbon self-doped nitrided carbon fibers: S4-1, firstly add dicyandiamide to the reactor in S3, heat it under a first temperature gradient under oscillation conditions, turn off the electric field after the reaction is completed, and finally volatilize the solvent and dry it to obtain a solid powder; the mass ratio of dicyandiamide to CNF-COOH is 4 to 6:1; The first temperature gradient is: first, uniformly heating from room temperature to 40°C within 3 to 5 minutes, and keeping warm for 1 to 2 minutes; then, uniformly heating from 40°C to 60°C within 3 to 5 minutes, and keeping warm for 2 to 3 minutes; then, uniformly heating from 60°C to 90°C within 1 to 2 minutes, and keeping warm for 9 to 10 hours; finally, naturally cooling to room temperature; The temperature at which the solvent evaporates is 55 to 65°C; S4-2, placing the solid powder prepared in S4-1 into a mixed atmosphere, and heating it under a second temperature gradient to obtain carbon self-doped carbon nitride fiber, which is recorded as g-C3N4 fiber; The volume ratio of nitrogen to air in the mixed atmosphere is 4 to 4.5:1; The second temperature gradient is: first, uniformly heating from room temperature to 50°C within 6 to 8 minutes, and keeping warm for 4 to 5 minutes; then, uniformly heating from 80°C to 100°C within 2 to 3 minutes, and keeping warm for 3 to 5 minutes; then, uniformly heating from 100°C to 300°C within 15 to 20 minutes, and keeping warm for 9 to 10 minutes; then, uniformly heating from 300°C to 500°C within 15 to 20 minutes, and keeping warm for 2 to 3 hours; finally, naturally cooling to room temperature; S5. Preparation of CoOOH / CN composite catalyst: First, add Co(NO3)2·6H2O solution to a reactor with parallel electrodes at the bottom; then add g-C3N4 fiber prepared by S4-2 and apply electric field, and ultrasonically treat for 25-35 minutes; then add NaOH solution and react at 45-50°C for 2-3 minutes; then add H2O2 and react at 45-55°C for 4.5-6 hours before turning off the electric field; finally, wash and dry the precipitate obtained after the reaction to obtain a composite fiber in which CoOOH is loaded on g-C3N4 fiber, i.e., CoOOH / CN composite catalyst; Let n be the multiplication number and n∈R + When the amount of g-C3N4 fiber added is n·1g, the amount of Co(NO3)2·6H2O solution added with a mass fraction of 20% is n·[40,60]mL, the amount of NaOH solution added with a mass fraction of 4% is n·[6,10]mL, and the amount of H2O2 added with a mass fraction of 30% is n·[4,8]mL.

2. The method for preparing a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination according to claim 1, characterized in that: The method for preparing carbon nanofibers described in S1 is: S1-1, firstly, add trimesic acid, zinc acetate dihydrate and DMF into a reactor, and stir evenly for 30-40 minutes to obtain a mixed solution; the concentration of trimesic acid in the mixed solution is 0.06-0.065 mmol / L, and the concentration of zinc acetate dihydrate is 0.18-0.20 mmol / L; S1-2, then the mixed solution in S1-1 is dynamically crystallized at 90-100° C. for 3-3.5 hours, and after the dynamic crystallization is completed, it is naturally cooled to room temperature to obtain a zinc-trimethylenetetracarboxylic acid metal organic framework, and the zinc-trimethylenetetracarboxylic acid metal organic framework is washed with DMF and then vacuum dried at 75-85° C. for 10-12 hours; S1-3, finally, the solid powder after vacuum drying in S1-2 is subjected to high temperature treatment under a third temperature gradient to obtain carbon nanofibers, which are recorded as CNF; The third temperature gradient is: first, uniformly increase the temperature from room temperature to 100°C within 8 to 10 minutes, and keep it warm for 4 to 5 minutes; then, uniformly increase the temperature from 100°C to 300°C within 8 to 10 minutes, and keep it warm for 3 to 5 minutes; then, uniformly increase the temperature from 300°C to 600°C within 10 to 15 minutes, and keep it warm for 1 to 1.5 minutes; then, uniformly increase the temperature from 600°C to 950°C within 10 to 15 minutes, and keep it warm for 2 to 3 hours; finally, naturally cool to room temperature.

3. The method for preparing a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination according to claim 1, characterized in that: The method for preparing carboxylated carbon nanofibers described in S2 is: S2-1, mixing concentrated sulfuric acid and concentrated nitric acid to prepare a mixed acid; S2-2, adding CNF and mixed acid prepared in S1 into the reactor successively, and ultrasonically treating at 40-50 kHz for 30-35 min; Let n be the multiplication number and n∈R + , when the amount of CNF added is n·1g, the amount of concentrated sulfuric acid with a mass fraction of 98% added is n·[30,33]mL, and the amount of concentrated nitric acid with a mass fraction of 65% added is n·[10,11]mL; S2-3, the product after ultrasonic treatment in S2-2 was stirred in a water bath at 80-90°C for 60-70 minutes, and naturally cooled to room temperature after the reaction; S2-4, dilute the product treated in S2-3 5 times with pure water, filter it with a microporous filter membrane with a pore size of 0.22 μm, and then wash and filter it repeatedly until the washed product is neutral; S2-5. The product washed to neutrality in S2-4 was dried under vacuum at 80° C. for 24 h to obtain carboxylated carbon nanofibers, which were recorded as CNF-COOH.

4. The method for preparing a carbon nitride-based catalyst for inhibiting photogenerated carrier recombination according to claim 1, characterized in that: The gap between the parallel electrodes in S3 is 3-5 μm, and the voltage amplitude of the AC voltage applied to the parallel electrodes is 10-15 V, and the frequency is 4-5 MHz.

5. Use of the carbon nitride-based catalyst for inhibiting photogenerated carrier recombination prepared by the preparation method according to claim 1, characterized in that: The CoOOH / CN composite catalyst is used to enhance the catalytic efficiency of peroxymonosulfate in a photoactivation process.