A p / m-FeS2 bicrystalline catalyst and its preparation method and application
By controlling the FeS2 crystal phase, a p/m-FeS2 bimorphic catalyst was prepared, which solved the problems of low conductivity and less exposed active sites of the existing p-FeS2 catalyst, significantly improved the activity of the oxidation electrolysis reaction, and achieved a better Efficient electrocatalytic performance.
Patent Information
- Application Number
- CN202410060855.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-01-16
AI Technical Summary
The existing p-FeS2 catalyst has poor oxidation electrolysis reaction (OER) activity due to its low intrinsic conductivity and less exposed active sites, and m-FeS2 has not been fully studied as an OER catalyst.
Using p/m-FeS2 bicrystal catalyst and its preparation method, the OER catalytic activity of the catalyst is controlled by controlling the FeS2 crystal phase, and specific chemical pretreatment and heat treatment steps are used to synthesize the bicrystal catalyst to improve its electrocatalytic performance.
The oxygen evolution reaction (OER) activity of water electrolysis is significantly improved. Compared with the single-phase p-FeS2 catalyst, its electrocatalytic performance is significantly improved, and the preparation process is simple and feasible.
Smart Images

Figure CN117926318B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalysis technology, and in particular to a p / m-FeS2 bicrystalline catalyst and a preparation method and application thereof. Background Art
[0002] As for FeS2 as an electrocatalytic oxygen evolution reaction (OER) catalyst, almost all literature reports are based on the research of the stable phase p-FeS2 (pyrite type), while m-FeS2 (marcasite type) with metastable characteristics and high conductivity as an OER catalyst is rarely reported. In addition, the reported p-FeS2 catalyst has poor OER activity due to its low intrinsic conductivity and less exposure of active sites. Therefore, in order to overcome the above shortcomings, it would be an effective method to regulate the OER catalytic activity of the catalyst by controlling the FeS2 crystal phase, because different crystal phases have different atomic structures and electronic properties, resulting in synergistic catalytic performance.
[0003] Therefore, a p / m-FeS2 bicrystalline catalyst and its preparation method and application are proposed to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a p / m-FeS2 bicrystalline catalyst and its preparation method and application. Not only is the preparation process simple, but the prepared p / m-FeS2 bicrystalline catalyst has good catalytic performance as an oxygen evolution electrocatalyst.
[0005] To achieve the above object, the present invention is implemented by adopting the following technical solutions:
[0006] A method for preparing a p / m-FeS2 bicrystalline catalyst comprises the following steps:
[0007] S1. Take 0.25-1.0mmol of Fe(NO3)2·9H2O and place it in a 100mL beaker. First, add 8mL of propylene glycol into the beaker with a syringe and stir for 3-5min. Then, add 40mL of isopropanol with a 50mL measuring cylinder and stir for a while with a magnetic stirrer to fully dissolve it to obtain a transparent orange-yellow solution A.
[0008] S2, transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor to react for a period of time, cool to room temperature, and then wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B;
[0009] S3. Take a 50mL beaker, add 20mL of anhydrous ethanol using a measuring cylinder, add 25-50mg of thioacetamide to the anhydrous ethanol, stir for 5-10min, and obtain a clear solution C;
[0010] S4, dispersing the solid B that has not been dried after centrifugation in the clear solution C, stirring it with a magnetic stirrer for a period of time to fully disperse it, and obtaining a suspension D;
[0011] S5, transfer the suspension D to an 80 mL reactor and react for a period of time, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, place in an oven to dry for a period of time, and obtain a black dry solid product E;
[0012] S6. Weigh 20-30 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1: (30-50) and place it on the other side of the magnetic boat.
[0013] S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon, heat it from room temperature to 350-500°C at a certain heating rate, and heat it at a constant temperature for a period of time to allow it to react fully. Allow it to cool naturally to room temperature to obtain p / m-FeS2 oxygen evolution electrocatalyst material.
[0014] Furthermore, in step S1, the rotation speed of the magnetic stirrer is 350 r / min, and the stirring time is 30 min.
[0015] Furthermore, in step S2, the reaction temperature of the high-pressure reactor is 180° C., and the reaction time is 6 hours.
[0016] Furthermore, in step S4, the rotation speed of the magnetic stirrer is 300 r / min, and the stirring time is 10-30 min.
[0017] Furthermore, in step S5, the reaction temperature of the high-pressure reactor is 160° C., and the reaction time is 1 h.
[0018] Furthermore, in step S5, the drying temperature of the oven is 60° C., and the drying time is 12 hours.
[0019] Furthermore, in step S7, the heating rate is 2-5°C / min.
[0020] Furthermore, the constant temperature heating time in step S7 is 4 hours.
[0021] The present invention also protects a p / m-FeS2 bi-crystalline catalyst.
[0022] The present invention also protects the use of p / m-FeS2 bi-crystalline catalyst as an oxygen evolution electrocatalyst.
[0023] The beneficial effects of the present invention are as follows:
[0024] 1. This method is used to synthesize p / m-FeS2. The method is simple and feasible, and the morphology is uniform and controllable.
[0025] 2. The p / m-FeS2 (dual-phase) catalyst prepared by this method has significantly improved oxygen evolution reaction (OER) activity in water electrolysis compared to the p-FeS2 (single-phase) catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the XRD diagram of the p / m-FeS2 material prepared in Examples 1-4 of the present invention.
[0027] Figure 2 This is the SEM image of the p / m-FeS2 material prepared in Example 1 of the present invention.
[0028] Figure 3 This is the TEM image of the p / m-FeS2 material prepared in Example 1 of the present invention.
[0029] Figure 4 This is a comparison chart of the OER performance of the p / m-FeS2 material prepared in Example 1 of the present invention and p-FeS2. DETAILED DESCRIPTION
[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0031] Example 1
[0032] A method for preparing a p / m-FeS2 bicrystalline catalyst comprises the following steps:
[0033] S1. Take 0.25mmol of Fe(NO3)2·9H2O and place it in a 100mL beaker. First, add 8mL of propylene glycol into the beaker with a syringe and stir for 3min. Then, add 40mL of isopropanol with a 50mL measuring cylinder. Use a magnetic stirrer to stir at a speed of 350r / min for 30min to fully dissolve it to obtain a transparent orange-yellow solution A.
[0034] S2. Transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor, react at 180° C. for 6 h, cool to room temperature, and wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B;
[0035] S3. Take a 50 mL beaker, add 20 mL of anhydrous ethanol using a measuring cylinder, add 25 mg of thioacetamide to the anhydrous ethanol, stir for 10 min, and obtain a clear solution C;
[0036] S4, dispersing the undried solid B after centrifugation in the clarified solution C, stirring with a magnetic stirrer at a speed of 300 r / min for 10 min to fully disperse it, and obtaining a suspension D;
[0037] S5. Transfer the suspension D to an 80 mL reactor, react at 160° C. for 1 h, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, and dry in an oven at 60° C. for 12 h to obtain a black dry solid product E.
[0038] S6. Weigh 20 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1:30 and place it on the other side of the magnetic boat.
[0039] S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon (the side of the magnetic boat containing sulfur powder is the air inlet), heat it from room temperature to 350°C at a heating rate of 5°C / min, and heat it at a constant temperature for 4 hours to allow it to react fully. Allow it to cool naturally to room temperature to obtain p / m-FeS2 oxygen evolution electrocatalyst material.
[0040] Example 2
[0041] A method for preparing a p / m-FeS2 bicrystalline catalyst comprises the following steps:
[0042] S1. Take 0.25mmol of Fe(NO3)2·9H2O and place it in a 100mL beaker. First, add 8mL of propylene glycol into the beaker with a syringe and stir for 5min. Then, add 40mL of isopropanol with a 50mL measuring cylinder. Use a magnetic stirrer to stir at a speed of 350r / min for 30min to fully dissolve it, and obtain a transparent orange-yellow solution A.
[0043] S2. Transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor, react at 180° C. for 6 h, cool to room temperature, and wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B;
[0044] S3. Take a 50 mL beaker, add 20 mL of anhydrous ethanol using a measuring cylinder, add 37.5 mg of thioacetamide to the anhydrous ethanol, stir for 10 min, and obtain a clear solution C;
[0045] S4, dispersing the undried solid B after centrifugation in the clarified solution C, stirring with a magnetic stirrer at a speed of 300 r / min for 10 min to fully disperse it, and obtaining a suspension D;
[0046] S5. Transfer the suspension D to an 80 mL reactor, react at 160° C. for 1 h, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, and dry in an oven at 60° C. for 12 h to obtain a black dry solid product E.
[0047] S6. Weigh 25 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1:35 and place it on the other side of the magnetic boat.
[0048] S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon (the side of the magnetic boat containing sulfur powder is the air inlet), heat it from room temperature to 400°C at a heating rate of 2°C / min, and heat it at a constant temperature for 4 hours to allow it to react fully. Allow it to cool naturally to room temperature to obtain p / m-FeS2 oxygen evolution electrocatalyst material.
[0049] Example 3
[0050] A method for preparing a p / m-FeS2 bicrystalline catalyst comprises the following steps:
[0051] S1. Take 0.5 mmol of Fe(NO3)2·9H2O and place it in a 100 mL beaker. First, add 8 mL of propylene glycol into the beaker with a syringe and stir for 5 min. Then, add 40 mL of isopropanol with a 50 mL measuring cylinder. Use a magnetic stirrer to stir at a speed of 350 r / min for 30 min to fully dissolve it, and obtain a transparent orange-yellow solution A.
[0052] S2. Transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor, react at 180° C. for 6 h, cool to room temperature, and wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B;
[0053] S3. Take a 50 mL beaker, add 20 mL of anhydrous ethanol using a measuring cylinder, add 37.5 mg of thioacetamide to the anhydrous ethanol, stir for 10 min, and obtain a clear solution C;
[0054] S4, dispersing the solid B that has not been dried after centrifugation in the clarified solution C, stirring it with a magnetic stirrer at a speed of 300 r / min for 20 min to fully disperse it, and obtaining a suspension D;
[0055] S5. Transfer the suspension D to an 80 mL reactor, react at 160° C. for 1 h, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, and dry in an oven at 60° C. for 12 h to obtain a black dry solid product E.
[0056] S6. Weigh 25 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1:40 and place it on the other side of the magnetic boat.
[0057] S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon (the side of the magnetic boat containing sulfur powder is the air inlet), heat it from room temperature to 450°C at a heating rate of 3°C / min, and heat it at a constant temperature for 4 hours to allow it to react fully. Allow it to cool naturally to room temperature to obtain p / m-FeS2 oxygen evolution electrocatalyst material.
[0058] Example 4
[0059] A method for preparing a p / m-FeS2 bicrystalline catalyst comprises the following steps:
[0060] S1. Take 1 mmol of Fe(NO3)2·9H2O and place it in a 100 mL beaker. First, add 8 mL of propylene glycol into the beaker with a syringe and stir for 5 min. Then, add 40 mL of isopropanol with a 50 mL measuring cylinder. Use a magnetic stirrer to stir at a speed of 350 r / min for 30 min to fully dissolve it, and obtain a transparent orange-yellow solution A.
[0061] S2. Transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor, react at 180° C. for 6 h, cool to room temperature, and wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B;
[0062] S3. Take a 50 mL beaker, add 20 mL of anhydrous ethanol using a measuring cylinder, add 50 mg of thioacetamide to the anhydrous ethanol, stir for 30 min, and obtain a clear solution C;
[0063] S4, dispersing the solid B that has not been dried after centrifugation in the clarified solution C, stirring it with a magnetic stirrer at a speed of 300 r / min for 30 min to fully disperse it, and obtaining a suspension D;
[0064] S5. Transfer the suspension D to an 80 mL reactor, react at 160° C. for 1 h, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, and dry in an oven at 60° C. for 12 h to obtain a black dry solid product E.
[0065] S6. Weigh 25 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1:50 and place it on the other side of the magnetic boat.
[0066] S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon (the side of the magnetic boat containing sulfur powder is the air inlet), heat it from room temperature to 500°C at a heating rate of 5°C / min, and heat it at a constant temperature for 4 hours to allow it to react fully. Allow it to cool naturally to room temperature to obtain p / m-FeS2 oxygen evolution electrocatalyst material.
[0067] from Figure 1 It can be seen that in step S7 of the preparation method, p / m-FeS2 materials can be obtained after the calcination temperature is set at 350, 400, 450, and 500°C for 4 hours, and their XRD contains p-FeS2 and m-FeS2 phases, respectively, proving that the p / m-FeS2 material is successfully synthesized.
[0068] from Figure 2 and Figure 3 It can be seen that the morphology of the p / m-FeS2 material prepared in Example 1 is spherical and evenly distributed; and the porous structure of the sample is conducive to electrolyte diffusion and accelerated mass transfer, thereby improving the electrocatalytic OER performance.
[0069] from Figure 4 It can be seen that the p / m-FeS2 material prepared in Example 1 has excellent OER performance when used as an oxygen evolution reaction electrocatalyst, and its OER performance is significantly improved compared with the p-FeS2 material.
[0070] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description. Therefore, it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention, and any figure marks in the claims should not be regarded as limiting the claims involved.
[0071] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A p / m-FeS 2 A method for preparing a bicrystalline catalyst, It is characterized in that The following steps are involved: S1, take 0.25-1.0mmol Fe(NO 3 ) 2 9H 2 O was placed in a 100 mL beaker, 8 mL of propylene glycol was first added into the beaker using a syringe and stirred for 3-5 min, then 40 mL of isopropanol was added using a 50 mL measuring cylinder, and stirred for a period of time using a magnetic stirrer to fully dissolve it, to obtain a transparent orange-yellow solution A; S2, transfer the transparent orange-yellow solution A to an 80 mL high-pressure reactor and react for a period of time, cool to room temperature, and then wash with anhydrous ethanol at 9000 r / min for 3 times to obtain solid B; S3. Take a 50mL beaker, add 20mL of anhydrous ethanol using a measuring cylinder, add 25-50mg of thioacetamide to the anhydrous ethanol, stir for 5-10min, and obtain a clear solution C; S4, dispersing the solid B that has not been dried after centrifugation in the clear solution C, stirring it with a magnetic stirrer for a period of time to fully disperse it, and obtaining a suspension D; S5, transfer the suspension D to an 80 mL reactor and react for a period of time, cool to room temperature, wash with anhydrous ethanol at 9000 r / min for 3 times, place in an oven to dry for a period of time, and obtain a black dry solid product E; S6. Weigh 20-30 mg of solid product E and grind it in an agate mortar for 10 min. Spread the ground powder evenly on one side of the magnetic boat. Based on the weight of the solid product E, weigh sulfur powder at a mass ratio of 1: (30-50) and place it on the other side of the magnetic boat. S7. Place the magnetic boat containing the solid product E and sulfur powder in a quartz tube filled with ultrapure argon, heat it from room temperature to 350-500°C at a certain heating rate, and heat it at a constant temperature for 4 hours to allow it to react fully, and then cool it naturally to room temperature to obtain p / m-FeS 2 Oxygen evolution electrocatalyst materials.
2. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: In step S1, the rotation speed of the magnetic stirrer is 350 r / min, and the stirring time is 30 min.
3. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: The reaction temperature of the high-pressure reactor in step S2 is 180° C., and the reaction time is 6 hours.
4. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: In step S4, the rotation speed of the magnetic stirrer is 300 r / min, and the stirring time is 10-30 min.
5. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: In the step S5, the reaction temperature of the high-pressure reactor is 160° C., and the reaction time is 1 hour.
6. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: In step S5, the drying temperature of the oven is 60° C. and the drying time is 12 hours.
7. A p / m-FeS according to claim 1 2 A method for preparing a bicrystalline catalyst, Features: The heating rate in step S7 is 2-5°C / min.
8. A p / m-FeS prepared by the preparation method according to any one of claims 1 to 7 2 Bicrystalline catalyst.