Composite catalyst, preparation method and its application in syngas to ethanol

By preparing a composite catalyst containing rhenium, iridium, and lanthanum, the problems of low conversion rate and poor selectivity of existing catalysts in the process of ethanol production from syngas were solved, achieving efficient ethanol production and long catalyst life, while reducing energy consumption.

CN117943051BActive Publication Date: 2026-11-17TANGSHAN ZHONGRONG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311802222.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Existing catalysts exhibit low conversion rates and poor ethanol selectivity in the process of producing ethanol from syngas, and also have short catalyst lifetimes, high energy consumption, and poor economic efficiency.

Method used

A composite catalyst, including rhenium oxide, iridium oxide and lanthanum oxide as the main catalyst, supplemented by nitrate-based co-catalysts and molybdenum dioxide as a support, is prepared by a specific method to form a highly dispersed active component solution, which is then precipitated and impregnated onto the support, and calcined to obtain the composite catalyst, which is used to produce ethanol from syngas.

Benefits of technology

It improves the conversion rate of syngas and the selectivity of ethanol, significantly enhances the catalyst's lifespan and economic efficiency, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a composite catalyst, its preparation method, and its application in the production of ethanol from syngas. The invention employs a precipitation method, where an alkaline solution is added dropwise to a mixed solution of rhenium, iridium, lanthanum, and an organic solvent to form a precipitate. A support is then added, and the mixture is stirred uniformly for a period of time to adsorb the precipitate onto the support. The precipitate is then filtered and washed to remove impurities, and finally dried and calcined to obtain the composite rhenium, iridium, and lanthanum catalyst. Under these conditions, the catalyst achieves optimal performance: a syngas conversion rate of 76.9% and a total alcohol selectivity of 61.4%, with approximately 95.3% of the alcohol products being ethanol and higher alcohols, and approximately 65.2% being ethanol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of syngas-to-ethanol technology, and in particular to a composite catalyst, its preparation method, and its application in syngas-to-ethanol production. Background Technology

[0002] Ethanol is currently the world's oldest and largest-volume fermentation industrial product, widely used in food, chemical, pharmaceutical, dye, and defense industries. It is also a crucial clean energy source, not only replacing tetraethyl lead as an anti-knock agent in gasoline but also enabling the production of ethanol gasoline, significantly reducing environmental pollution from gasoline combustion. Its future market prospects are extremely broad. my country has made initial progress in ethanol synthesis technology using hydrogenation, but many problems remain to be solved during industrialization, such as: unstable quality of hydrogenation catalysts, poor catalytic effect, and short lifespan; high energy consumption and low overall energy utilization rate in the production process; and high cost of hydrogen sources, resulting in poor project economics.

[0003] There are three main types of catalysts for syngas-to-ethanol production: rhodium-based catalysts, molybdenum-based catalysts, and copper-based catalysts. Rhodium-based catalysts exhibit high ethanol synthesis performance, but the precious metal rhodium limits their industrial application. Molybdenum-based catalysts are primarily modified MoS2 catalysts; these catalysts require harsh reaction conditions and produce products predominantly composed of hydrocarbons. Currently, metal-modified copper-based catalysts are the most frequently reported, but they produce products with a high methanol content and less desirable ethanol composition.

[0004] The catalytic synthesis of ethanol from syngas is a complex reaction involving multiple elementary reactions and the presence of CO molecule dissociation and non-dissociation centers. The rate matching between the carbon chain growth process and the CO insertion process is a key factor in obtaining more ethanol and higher alcohols. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing catalyst systems, such as low syngas conversion rate and poor ethanol selectivity, and to provide a composite catalyst, a preparation method, and its application in the production of ethanol from syngas.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] One aspect of the present invention provides a composite catalyst. The composite catalyst comprises a main catalyst, a promoter, and a support. The main catalyst comprises rhenium oxide, iridium oxide, and lanthanum oxide; the promoter is selected from one or more of copper nitrate, cobalt nitrate, nickel nitrate, copper chloride, cobalt chloride, or nickel chloride; the support comprises one or more of molybdenum dioxide, titanium dioxide, cerium dioxide, zirconium dioxide, or silicon carbide; the composite catalyst contains 0.3-5% rhenium by mass, 0-2% iridium by mass, and 0-1.5% lanthanum by mass.

[0008] Furthermore, the carrier is preferably zirconium dioxide.

[0009] The second aspect of this invention provides a method for preparing the composite catalyst, comprising the following steps:

[0010] S1: Dissolve rhenium precursor, iridium precursor and lanthanum precursor in an organic solution at a ratio of 1g:1g:1g to prepare a 0.02-0.2mol / L mixed solution. Disperse the mixed solution by ultrasonication to obtain a highly dispersed active component solution.

[0011] S2: Add the alkaline solution dropwise to the above-mentioned component solution to form a precipitate. Add the support to the solution where the precipitate is formed and stir. Add the catalyst to impregnate the precipitate onto the support. The support accounts for 10-20% of the total mass of the system after addition. Separate the liquid and solid by centrifugation, remove the supernatant, leave the solid part, and dry it to obtain the composite rhenium, iridium, and lanthanum catalyst precursor.

[0012] S3: Wash the above-mentioned composite rhenium, iridium, and lanthanum catalyst precursor with an organic solvent until the organic solution is colorless, remove the organic solvent, dry, and calcine to obtain the composite rhenium, iridium, and lanthanum catalyst.

[0013] Further, the rhenium precursor mentioned in step S1 is one or more of ReCl3, ReCl(PPh3)3, and HRe(PPh3)3; the iridium precursor is one or more of IrCl3, IrCl(PPh3)3, and HIr(PPh3)3; and the lanthanum precursor is one or more of LaCl3, LaCl(PPh3)3, and HLa(PPh3)3.

[0014] Furthermore, the rhenium precursor is preferably ReCl(PPh3)3; the iridium precursor is preferably IrCl(PPh3)3; and the lanthanum precursor is preferably LaCl(PPh3)3.

[0015] Further, the organic solvent mentioned in step S1 is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylaniline, acetylacetone, and butyronitrile.

[0016] Further, the alkaline solution mentioned in step S2 is one or more of sodium hydroxide, potassium hydroxide, and calcium hydroxide.

[0017] Furthermore, the immersion temperature in step S2 is 35-75°C, and the immersion time is 24-36 hours.

[0018] Further, the organic solvent in step S3 is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylaniline, acetylacetone, and butyronitrile.

[0019] Furthermore, the calcination temperature in step S3 is 400-800℃, and the heating rate is 0.1-5℃ / min.

[0020] The third aspect of this invention provides the application of the composite rhenium, iridium, and lanthanum catalyst prepared according to the aforementioned method in the synthesis of ethanol from syngas.

[0021] Using CO and H2 as raw materials, a composite catalyst is added, and a certain proportion of CO and H2 synthesis gas is introduced, under conditions of 10-20 MPa pressure, 350-420℃ temperature, and gas space velocity of 2000-4000 h⁻¹. -1 The reaction proceeds to obtain ethanol with a high content.

[0022] Furthermore, the synthesis gas V(H2) / V(CO) = 0.5-2.

[0023] Compared with the prior art, the advantages of the present invention are that it overcomes the disadvantages of existing catalyst systems such as low syngas conversion rate and poor ethanol selectivity. Detailed Implementation

[0024] The present invention will now be described in detail with reference to specific embodiments. Unless otherwise specified, all raw materials used in this invention are commercially available or can be prepared using conventional methods in the art. The fixed bed used in this patent is prior art in the art.

[0025] Example 1

[0026] Accurately weigh 0.1 g ReCl(PPh3)3, 0.1 g IrCl(PPh3)3, and 0.1 g LaCl(PPh3)3 and add them to 5 mL of N,N-dimethylacetamide solution to prepare a 0.05 mol / L solution, which is then placed in a 100 mL beaker. Place the beaker in an ultrasonic cleaner and disperse at 40 kHz for 30–60 min to obtain a highly dispersed active component solution. Add 120 mL each of 0.1 M sodium hydroxide and potassium hydroxide to 65 mL of the active component solution to form precipitates. Add 5 g TiO2 support to the precipitated active component solution, then add 10 g of copper nitrate and 10 g of cobalt nitrate as catalyst promoters. After impregnation at room temperature for 28 h, centrifuge to remove the liquid to obtain the composite rhenium, iridium, and lanthanum catalyst precursor. The composite rhenium, iridium, and lanthanum catalyst precursor was dried at 80°C for 6 hours, washed repeatedly with N,N-dimethylacetamide solution, dried at 80°C for 6 hours, and then heated to 550°C in a muffle furnace at a heating rate of 5°C / min and held at that temperature for 36 hours to obtain the composite rhenium, iridium, and lanthanum catalyst. The prepared composite rhenium, iridium, and lanthanum catalyst was granulated by pressing into tablets, and the total percentage of rhenium, iridium, and lanthanum in the composite catalyst was 2.7%.

[0027] The catalyst performance was evaluated in a fixed-bed reactor. Reaction conditions: temperature 400℃, pressure 12MPa, space velocity 2500h⁻¹. -1 The syngas V(H2) / V(CO) ratio is 0.9. Gas chromatography yielded a syngas conversion rate of 63.5% and a total alcohol selectivity of 46.7%, with ethanol and higher alcohols comprising 74.2% and ethanol content of 32.8%.

[0028] Example 2

[0029] The method is the same as in Example 1, except that 0.1g ReCl(PPh3)3, 0.1g IrCl(PPh3)3, and 0.1g LaCl(PPh3)3 are added to 5mL of acetonitrile solution to prepare a 0.05mol / L solution, thereby preparing a composite rhenium, iridium, and lanthanum catalyst. The total percentage of rhenium, iridium, and lanthanum in the composite catalyst is 3.1%.

[0030] The results were evaluated according to the evaluation method in Example 1: syngas conversion rate was 68.3%, total alcohol selectivity was 50.1%, of which ethanol and higher alcohol content was 76.1%, and ethanol content was 37.8%.

[0031] Example 3

[0032] The technical solution and evaluation method are the same as in Example 1, except that 0.1g ReCl(PPh3)3, 0.1g IrCl(PPh3)3, and 0.1g LaCl(PPh3)3 are added to 5mL of acetylacetone solution to prepare a 0.05mol / L solution, thereby preparing a composite rhenium, iridium, and lanthanum catalyst.

[0033] The results were evaluated according to the evaluation method in Example 1: syngas conversion rate was 70.4%, total alcohol selectivity was 51.2%, of which ethanol and higher alcohol content was 84.1%, and ethanol content was 38.6%.

[0034] Example 4

[0035] The technical solution and evaluation method are the same as in Example 1, except that 5g of MoO2 support is added to the active component solution to prepare a composite rhenium, iridium and lanthanum catalyst, and the total percentage of rhenium, iridium and lanthanum in the composite catalyst is 3.2%.

[0036] The results were evaluated according to the evaluation method in Example 1: syngas conversion rate was 68.7%, total alcohol selectivity was 50.1%, of which ethanol and higher alcohol content was 80.4%, and ethanol content was 36.9%.

[0037] Example 5

[0038] The technical solution and evaluation method are the same as in Example 1, except that 5g of SiC support is added to the active component solution to prepare a composite rhenium, iridium, and lanthanum catalyst, and the total percentage of rhenium, iridium, and lanthanum in the composite catalyst is 3.7%.

[0039] The results were evaluated according to the evaluation method in Example 1: syngas conversion rate was 74.2%, total alcohol selectivity was 60.3%, of which ethanol and higher alcohol content was 94.1%, and ethanol content was 63.5%.

[0040] Example 6

[0041] The technical solution and evaluation method are the same as in Example 1, except that 5g of ZrO2 support is added to the active component solution to prepare a composite rhenium, iridium and lanthanum catalyst, and the total percentage of rhenium, iridium and lanthanum in the composite catalyst is 3.9%.

[0042] The results were evaluated according to the evaluation method in Example 1: syngas conversion rate was 73.6%, total alcohol selectivity was 60.4%, of which ethanol and higher alcohol content was 94.7%, and ethanol content was 62.8%.

[0043] Comparative Example 1

[0044] The technical solution and evaluation method are the same as in Example 1, except that 0.1g ReCl(PPh3)3 and 0.1g IrCl(PPh3)3 are weighed and added to 5mL of N,N-dimethylacetamide solution to prepare a 0.05mol / L solution, thereby preparing a composite rhenium-iridium catalyst. The total percentage of rhenium and iridium in the composite catalyst is 2.7%.

[0045] The results were evaluated according to the evaluation method of Example 1: syngas conversion rate was 60.1%, total alcohol selectivity was 41.3%, of which ethanol and higher alcohol content was 67.2%, and ethanol content was 28.3%.

[0046] Comparative Example 2

[0047] The technical solution and evaluation method are the same as in Example 1, except that 0.1g ReCl(PPh3)3 and 0.1g LaCl(PPh3)3 are weighed and added to 5mL of N,N-dimethylacetamide solution to prepare a 0.05mol / L solution, thereby preparing a composite rhenium and lanthanum catalyst. The total percentage of rhenium and lanthanum in the composite catalyst is 2.9%.

[0048] The results were evaluated according to the evaluation method of Example 1: syngas conversion rate was 62.7%, total alcohol selectivity was 40.3%, of which ethanol and higher alcohol content was 68.1%, and ethanol content was 28.4%.

[0049] It can be seen that the syngas conversion rate and total alcohol selectivity of the binary composite catalyst are lower than those of the syngas conversion rate and total alcohol selectivity of the ternary composite catalyst prepared in this invention in the preparation of ethanol.

[0050] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A composite catalyst, characterized in that, The composite catalyst comprises a main catalyst, a promoter, and a support; wherein the main catalyst comprises rhenium oxide, iridium oxide, and lanthanum oxide; the promoter is selected from copper nitrate and cobalt nitrate; the support is SiC or ZrO2; the mass percentage of rhenium in the composite catalyst is 0.3-5%, the mass percentage of iridium is 0-2% and not 0, and the mass percentage of lanthanum is 0-1.5% and not 0; The total percentage of rhenium, iridium, and lanthanum in the composite catalyst is 3.7% or 3.9%.

2. A method for preparing the composite catalyst as described in claim 1, characterized in that, Includes the following steps: S1: Rhenium precursor, iridium precursor and lanthanum precursor are dissolved in an organic solution at a ratio of 1:1:1 to prepare a 0.05 mol / L mixed solution. The mixed solution is ultrasonically dispersed to obtain a highly dispersed active component solution. S2: Add the alkaline solution dropwise to the above active component solution to form a precipitate, add the support to the solution where the precipitate is formed and stir, add a catalyst promoter to impregnate the precipitate onto the composite catalyst support, and centrifuge to dry the solid part to obtain the composite rhenium, iridium and lanthanum catalyst precursor; S3: Wash the above-mentioned composite rhenium, iridium, and lanthanum catalyst precursor with an organic solvent until the organic solution is colorless, remove the organic solvent, dry, and calcine to obtain the composite catalyst. The calcination conditions are: heating at a rate of 5 °C / min to 550 °C and holding at that temperature for 36 h. The rhenium precursor mentioned in step S1 is ReCl(PPh3)3; the iridium precursor is IrCl(PPh3)3; and the lanthanum precursor is LaCl(PPh3)3.

3. The method for preparing a composite catalyst according to claim 2, characterized in that, The organic solvent mentioned in step S1 is N,N-dimethylacetamide.

4. The method for preparing a composite catalyst according to claim 2, characterized in that, The alkaline solution in step S2 is a mixture of sodium hydroxide and potassium hydroxide; the concentration of the alkaline solution is 0.1 M, and the ratio of the alkaline solution to the active component solution is 120 mL: 65 mL.

5. The method for preparing a composite catalyst according to claim 2, characterized in that, The organic solvent in step S3 is N,N-dimethylacetamide.

6. The application of the composite catalyst as described in claim 1 in the preparation of ethanol from syngas, specifically, the application method is as follows: using CO and H2 as raw materials, adding the composite catalyst, and introducing CO and H2 syngas, with syngas V(H2) / V(CO) = 0.9, at a pressure of 12 MPa, a temperature of 400 °C, and a gas space velocity of 2500 h⁻¹. -1 The reaction proceeds to yield ethanol.

Citation Information

Patent Citations

  • Composite carrier type catalyst for preparing low-carbon alcohol from synthesis gas, and preparation method thereof

    CN110898847A

  • Production of alcohols from synthesis gas

    GB2078745A