Ir / Mo2C / C composite material and preparation method and application thereof
By using Ir/Mo2C/C composite material as the anode catalyst for alkaline membrane fuel cells, the problems of poor catalyst stability and high cost were solved, achieving a highly efficient alkaline hydroxide reaction and improving the performance and durability of the fuel cell.
Patent Information
- Application Number
- CN202410177677.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-02-08
AI Technical Summary
Existing alkaline membrane fuel cells have poor anode catalyst stability and high platinum group metal loading, leading to increased costs and insufficient activity.
An Ir/Mo2C/C composite material was used as a catalyst, in which Ir was distributed in a single-atom dispersion state on a Mo2C support with a loading of 1-15 wt%. The composite material was prepared by a specific preparation method.
This improved the stability of the catalyst and its alkaline hydrogen oxidation activity, reduced the loading of platinum group metals, and significantly enhanced the performance and durability of the fuel cell.
Smart Images

Figure CN117996092B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite materials, and in particular to an Ir / Mo2C / C composite material and a preparation method and application thereof. Background Art
[0002] At present, the excessive use of traditional fossil energy has caused unprecedented pollution to the earth's environment. In order to meet human energy needs while protecting the environment, various countries have launched a wave of research on new energy.
[0003] The use of hydrogen energy provides a viable solution to reduce dependence on fossil fuels and environmental protection issues. Fuel cells play a vital role in establishing a hydrogen economy.
[0004] Alkaline membrane fuel cells (HEMFCs) are similar to proton exchange membrane fuel cells (PEMFCs), and the ion exchange membrane they use is an anion exchange membrane. Since alkaline membrane fuel cells can use non-platinum group metal cathode electrocatalysts (such as Ag, Mn-Co oxides and Fe-NC, etc.) and nickel-based bipolar plates, they have good development prospects.
[0005] At present, the anode catalysts of high-performance proton exchange membrane fuels still rely on platinum group metals. When the electrolyte changes from acidic to alkaline, its hydrogen oxidation reaction (HOR) kinetics slow down significantly by about 2-3 orders of magnitude, resulting in a higher platinum group metal loading on the anode of the alkaline membrane fuel cell. Therefore, the anode cost of the alkaline membrane fuel cell will also increase significantly. In addition, HEMFCs that generally use platinum-based catalysts have poor stability and require higher catalyst loadings to drive stable HEMFCs, further increasing costs.
[0006] Therefore, developing catalysts with high efficiency and stable catalytic ability while reducing the platinum group element loading on the anode of the alkaline hydrogen oxidation reaction is a key goal for the continued development of alkaline membrane fuel cells. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of low stability and poor reaction activity of alkaline hydrogen oxidation reaction catalysts in the prior art.
[0008] In order to achieve the above object, the first aspect of the present invention provides an Ir / Mo2C / C composite material, wherein the composite material contains a carrier and a metal active component, wherein the carrier contains Mo2C and carbon; the metal active component is Ir; and the metal active component is distributed on the Mo2C in a single-atom dispersed state;
[0009] Based on the total weight of the Ir / Mo2C / C composite material, the loading amount of the metal active component is 1-15wt%.
[0010] The second aspect of the present invention provides the use of the Ir / Mo2C / C composite material described in the first aspect in a hydrogen oxidation reaction catalyst.
[0011] The third aspect of the present invention provides a method for preparing the Ir / Mo2C / C composite material according to the first aspect, comprising:
[0012] (1) In the presence of water, a metal source and a carrier precursor are contacted and mixed and then evaporated to obtain an intermediate I;
[0013] (2) heating the intermediate I under a protective atmosphere to obtain the Ir / Mo2C / C composite material;
[0014] The metal source is a soluble compound capable of providing a metal active component, and the metal active component is Ir;
[0015] The carrier precursor is MoO x / C complex;
[0016] The metal active component can be distributed on the Mo2C in a single-atom dispersed state; based on the total weight of the Ir / Mo2C / C composite material, the amount of the metal source is such that the loading amount of the metal active component is 1-15wt%.
[0017] The present invention has at least the following advantages over the prior art:
[0018] The Ir / Mo2C / C composite material provided by the invention has excellent stability and alkaline hydrogen oxidation activity as an anode catalyst of an alkaline membrane fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is the TEM image of M1 obtained in Example 1 of the present invention (eg Figure 1 a and b in the figure), XRD (as shown in Figure 1 c), HAADF-STEM (as shown in Figure 1 d in the figure) and EDS mapping (as shown in Figure 1 d in the figure).
[0020] Figure 2 These are the polarization curves of M1 obtained in Example 1, commercially available Pt / C, commercially available PtRu / C, Ir / C obtained in Comparative Example 1, and Mo2C / C obtained in Comparative Example 2 tested in 0.1M KOH saturated with hydrogen.
[0021] Figure 3 is based on Figure 2Comparison of the mass ratio exchange current calculated from the polarization curves of M1, Ir / C, Pt / C and PtRu / C materials and the activity of the corresponding metal nanoparticles.
[0022] Figure 4 It is a performance diagram of an alkaline membrane fuel cell with low anode catalyst loading assembled with M1 obtained in Example 1, commercially available Pt / C, commercially available PtRu / C, and Ir / C obtained in Comparative Example 1.
[0023] Figure 5 yes Figure 4 Peak power density and mass activity diagram of materials for fuel cells shown in.
[0024] Figure 6 These are the chronoamperometric curves of M1 obtained in Example 1, M3 obtained in Example 3, Ir / C obtained in Comparative Example 1, commercially available Pt / C, and commercially available PtRu / C, obtained by testing at a constant potential of 50 mV at a rotation speed of 900 rpm in hydrogen-saturated 0.1 M KOH.
[0025] Figure 7 yes Figure 6 The stability of the potentiostatic test shown in .
[0026] Figure 8 is M1 obtained in Example 1 (such as Figure 8 As shown in a), commercially available PtRu / C (such as Figure 8 As shown in b), commercially available Pt / C (such as Figure 8 c in the figure), the Ir / C obtained in the comparative example (as shown in Figure 8 (d) Durability test (ADT) performed in hydrogen-saturated 0.1 M KOH at a scan rate of 2 mV / s in the range of 0 to 0.5 V.
[0027] Fig. 9 It is an accelerated durability analysis chart of M1 obtained in Example 1, Ir / C obtained in Comparative Example 1, commercially available Pt / C, and commercially available PtRu / C. DETAILED DESCRIPTION
[0028] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0029] The solubility mentioned in the present invention means being soluble in a solvent, such as water.
[0030] As mentioned above, the first aspect of the present invention provides an Ir / Mo2C / C composite material, wherein the composite material contains a carrier and a metal active component, wherein the carrier contains Mo2C and carbon; the metal active component is Ir; and the metal active component is distributed on the Mo2C in a single-atom dispersed state;
[0031] Based on the total weight of the Ir / Mo2C / C composite material, the loading amount of the metal active component is 1-15wt%.
[0032] The inventors of the present invention have found that the metal active components of the present invention are distributed on the Mo2C of the carrier in a single-atom dispersed state, so that the effective catalytic active sites are increased, which can effectively enhance the alkaline hydrogen oxidation activity of the Ir / Mo2C / C composite material.
[0033] Preferably, the loading amount of the metal active component is 1-5wt% based on the total weight of the Ir / Mo2C / C composite material. The inventors of the present invention have found that in this preferred case, the Ir / Mo2C / C composite material provided by the present invention has better stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst.
[0034] Preferably, the molar ratio of Ir to Mo in the Ir / Mo2C / C composite material is 1:5-15. The inventors of the present invention have found that in this preferred case, the Ir / Mo2C / C composite material provided by the present invention has better stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst.
[0035] In the Ir / Mo2C / C composite material of the present invention, the metal active component is distributed on the Mo2C in the carrier in a single-atom dispersed state, and the loading amount of the metal active component is 1-15wt%, preferably 1-5wt%; the elemental molar ratio of Ir and Mo in the composite material is 1:5-15; the balance is carbon.
[0036] Preferably, the average particle size of Mo2C loaded with the metal active component is 2-3 nm.
[0037] The second aspect of the present invention provides the use of the Ir / Mo2C / C composite material described in the first aspect in a hydrogen oxidation reaction catalyst.
[0038] The third aspect of the present invention provides a method for preparing the Ir / Mo2C / C composite material according to the first aspect, comprising:
[0039] (1) in the presence of water, a metal source and a carrier precursor are contacted and mixed and then evaporated to obtain an intermediate I;
[0040] (2) heating the intermediate I under a protective atmosphere to obtain the Ir / Mo2C / C composite material;
[0041] The metal source is a soluble compound capable of providing a metal active component, and the metal active component is Ir;
[0042] The carrier precursor is MoO x / C complex;
[0043] The metal active component can be distributed on the Mo2C in a single-atom dispersed state; based on the total weight of the Ir / Mo2C / C composite material, the amount of the metal source is such that the loading amount of the metal active component is 1-15wt%.
[0044] Preferably, in step (1), the metal source is IrCl3·xH2O and / or iridium acetylacetonate.
[0045] According to a preferred embodiment, in step (1), the contact mixing conditions include: temperature of 20-30° C. and time of 0.5-1.5 h.
[0046] More preferably, the contact mixing is performed under ultrasonic conditions.
[0047] Preferably, the frequency of the ultrasound is 30kHz-50kHz.
[0048] Preferably, in step (1), the conditions of the evaporation treatment include: temperature of 40-60°C, time of 0.5-1h, and pressure of -0.1Mpa to -0.05Mpa.
[0049] Preferably, in step (2), the conditions of the heating treatment include: a temperature of 500-1000° C. and a time of 0.5-1.5 h.
[0050] According to a preferred embodiment, the heating treatment is carried out at a heating rate of 8-12°C / min to 500-1000°C. The inventors of the present invention have found that in this preferred embodiment, the Ir / Mo2C / C composite material provided by the present invention has better stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst.
[0051] Preferably, in step (2), the protective atmosphere is selected from at least one of nitrogen, carbon dioxide and argon.
[0052] Further preferably, the protective atmosphere is a nitrogen atmosphere. The inventors of the present invention have found that in this preferred case, the Ir / Mo2C / C composite material provided by the present invention has better stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst.
[0053] Preferably, in step (2), before the heating treatment, the intermediate I is first ground to an average particle size of 0.07-0.1 mm. The inventors of the present invention have found that in this preferred case, the Ir / Mo2C / C composite material provided by the present invention has better stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst.
[0054] The present invention has no particular requirements on the specific operation methods and conditions of the evaporation treatment in step (1) and the grinding in step (2), and can be carried out by methods known in the art. The present invention will not be repeated here, and those skilled in the art should not interpret it as limiting the present invention.
[0055] Further preferably, the method further comprises preparing the MoO x / C complex:
[0056] (S1) dispersing carbon oxide powder, molybdenum pentachloride and a dispersant to obtain material A;
[0057] (S2) in the presence of water, subjecting the material A to a heat-insulating reaction to obtain material B;
[0058] (S3) freeze-drying the material B to obtain the MoO x / C complex.
[0059] Preferably, in step (S1), the dispersant is selected from at least one of ethanol, isopropanol and methanol. Particularly preferably, the dispersant is ethanol.
[0060] According to a preferred embodiment, in step (S1), the conditions of the dispersion reaction include: time of 10-20 min, temperature of 20-30°C.
[0061] Further preferably, the dispersion reaction is carried out under ultrasonic conditions.
[0062] Preferably, the frequency of the ultrasound is 30kHz-50kHz.
[0063] Preferably, in step (S2), the conditions for the heat preservation and heating reaction include: temperature of 80-100°C and time of 6-10h.
[0064] Preferably, the heat preservation and heating reaction is carried out under stirring conditions.
[0065] More preferably, the stirring speed is 200-300 rpm.
[0066] According to a preferred embodiment, in step (S3), before the freeze-drying treatment, the material B is first dispersed in water and filtered.
[0067] Further preferably, the freeze-drying treatment conditions include: a temperature of -60°C to -75°C and a time of 10-12 hours.
[0068] The present invention has no particular requirements on the specific operating methods and conditions of the stirring in step (S1) and the dispersing, filtering and freeze-drying in step (S3), and can be carried out by methods known in the art. The present invention will not be described in detail herein, and those skilled in the art should not interpret this as a limitation of the present invention.
[0069] According to a particularly preferred embodiment, the oxidized carbon powder is a product prepared by the following steps, including:
[0070] (X1) contacting a carbon raw material with a strong acid solution at a temperature of 50-100° C., and separating and treating a material I obtained after the contact reaction to obtain a carbon oxide precursor material;
[0071] (X2) The carbon oxide precursor material is dispersed in water and filtered, and the obtained carbon material is freeze-dried to obtain the carbon oxide powder.
[0072] Preferably, in step (X1), the strong acid solution is nitric acid and / or sulfuric acid. Particularly preferably, the strong acid is nitric acid.
[0073] Preferably, before the contact reaction, the carbon raw material and the strong acid solution are first subjected to ultrasonic pretreatment, and then the mixed solution obtained after the pretreatment is subjected to the contact reaction.
[0074] Further preferably, the frequency of the ultrasound is 30kHz-50kHz.
[0075] Preferably, in step (X1), the contact reaction temperature is 70-90°C and the time is 0.5-1.5h.
[0076] Preferably, in step (X1), the separation treatment is performed by centrifugal separation.
[0077] According to a preferred embodiment, the centrifugal separation conditions include: a rotation speed of 10500-11500 rpm and a time of 1-5 min.
[0078] Preferably, in step (X2), the freeze-drying treatment includes: a temperature of -75°C to -65°C and a time of 11-13 hours.
[0079] The present invention has no particular requirements on the specific operating methods and conditions of the freeze-drying and the filtration in step (X2), and can be carried out by methods known in the art. The present invention will not be described in detail herein, and those skilled in the art should not interpret this as a limitation of the present invention.
[0080] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all the raw materials and instruments used are commercially available.
[0081] Carbon raw material: Model KB-300J: purchased from Lion Corporation.
[0082] Metal source: IrCl3·xH2O, purchased from Sigma Aldrich.
[0083] Pt / C: Model Pt / C (mass fraction of Pt is 20 wt%), purchased from Johnson Matthey Company, USA.
[0084] PtRu / C: Model PtRu / C (mass fraction of Pt is 40 wt %, mass fraction of Ru is 20 wt %), purchased from Johnson Matthey Company, USA.
[0085] Catalyst characterization
[0086] The morphology of the prepared Ir / Mo2C / C composites was analyzed using a HITACHI HT7700 transmission electron microscope.
[0087] A FEI-Titan Cubed Themis G2300 scanning transmission electron microscope was used to characterize the atomic-scale structure of the Ir / Mo2C / C composites.
[0088] The composition of Ir / Mo2C / C composites was determined by Thermo-Fisher ICPS-6300 inductively coupled plasma optical emission spectrometer.
[0089] The CHI 760e electrochemical workstation was used to test the hydrogen oxidation reaction of the corresponding Ir / Mo2C / C composites.
[0090] The Scribner 850e battery system was used to test the performance of alkaline membrane fuel cells.
[0091] Preparation of oxidized carbon powder
[0092] Preparation Example 1
[0093] I. Weigh 1 g of KB-300J and disperse it in 100 mL of 65 wt% nitric acid. Ultrasonicate at 25°C for 30 min (ultrasonic frequency is 40 kHz) to obtain a mixed solution. Then place the mixed solution in an oil bath and react at 80°C for 1 h.
[0094] II. Pour the solution after the reaction in step I into a centrifuge tube, centrifuge at 11000 rpm for 3 min, then wash three times with ultrapure water, and dissolve the resulting carbon in 150 mL of ultrapure water;
[0095] III. Filter the mixed solution obtained in step II;
[0096] IV. The filter residue obtained in step III is freeze-dried in a freeze dryer (temperature is -70°C, time is 12 hours) to obtain oxidized carbon powder.
[0097] MoO x / C Preparation Example
[0098] Preparation Example 2
[0099] This preparation example is used to obtain MoO x / C, specifically:
[0100] 380 mg of MoCl5 and 200 mg of the oxidized carbon powder prepared in Preparation Example 1 were dissolved in a conical flask containing 30 ml of ethanol, and ultrasonicated at 25°C for 15 min (ultrasonic frequency was 40 kHz), then 5 ml of water was added, and then the mixed solution was heated to 80°C and stirred for 8 h (stirring speed was 250 rpm), and after cooling, the mixed solution was centrifuged, washed with a large amount of water, and then freeze-dried (temperature was -70°C, time was 12 h) to obtain MoO x / C composite powder, named Z2.
[0101] Preparation Example 3
[0102] The difference between this preparation example and preparation example 2 is that the content of MoCl5 is different, specifically:
[0103] 760 mg of MoCl5 and 200 mg of the oxidized carbon powder prepared in Preparation Example 1 were dissolved in a conical flask containing 30 ml of ethanol, and ultrasonicated at 25°C for 15 min (ultrasonic frequency was 40 kHz), followed by adding 5 ml of water, and then the mixed solution was heated to 80°C and stirred vigorously for 8 h (the stirring speed was the same as in Preparation Example 2), and after cooling, the mixed solution was centrifuged, washed with a large amount of water, and then freeze-dried (temperature was -70°C, time was 12 h) to obtain MoOx / C composite powder, named Z3.
[0104] Example 1
[0105] (1) 12 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z2) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time: 1 h, pressure: -0.1 MPa), and the residue was collected and dried overnight.
[0106] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The obtained sample was an Ir / Mo2C / C composite material, named M1.
[0107] Example 2
[0108] This example uses a method and process conditions similar to those of Example 1 to prepare an Ir / Mo2C / C composite material, except that the amount of the metal source is different, specifically:
[0109] (1) 18.75 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z2) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0110] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The resulting sample was an Ir / Mo2C / C composite material, named M2.
[0111] Example 3
[0112] This example uses a method and process conditions similar to those of Example 1 to prepare an Ir / Mo2C / C composite material, except that the amount of the metal source is different, specifically:
[0113] (1) 37.5 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z2) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0114] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The obtained sample was an Ir / Mo2C / C composite material, named M3.
[0115] Example 4
[0116] This embodiment adopts a method and process conditions similar to those of embodiment 1 to prepare the Ir / Mo2C / C composite material, except that the temperature in step (2) is adjusted to 500°C. Specifically:
[0117] (1) 12 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z2) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0118] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 500°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The resulting sample was an Ir / Mo2C / C composite material, named M4.
[0119] Example 5
[0120] This embodiment adopts a method and process conditions similar to those of embodiment 1 to prepare the Ir / Mo2C / C composite material, except that the temperature in step (2) is adjusted to 700°C. Specifically:
[0121] (1) 12 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z2) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0122] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 700°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The obtained sample was an Ir / Mo2C / C composite material, named M5.
[0123] Example 6
[0124] This example uses a method and process conditions similar to those of Example 1 to prepare an Ir / Mo2C / C composite material, except that Z2 is replaced by Z3 ( The molar ratio of Ir and Mo in Ir / Mo2C / C was adjusted from 1:10 to 1:20 ), specifically:
[0125] (1) 12 mg of IrCl3·xH2O (metal source) and 109 mg of MoOx / C powder (type Z3) were dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0126] (2) The intermediate obtained in step (1) was ground into an average particle size of 0.1 mm using a mortar, and then spread flat on a magnetic boat. The magnetic boat was placed in a quartz tube, and heated to 900°C at a heating rate of 10°C / min under a nitrogen atmosphere, and maintained at this condition for 1 h. The obtained sample was an Ir / Mo2C / C composite material, named M6.
[0127] The distinguishing features of Examples 1 to 6 are summarized in Table 1;
[0128] Table 1
[0129] Example No. Ir load Molar ratio of Ir to Mo Metal source dosage / mg First reaction temperature / ℃ 1 3.2wt% 1:10 12 900 2 5wt% 1:10 18.75 900 3 10wt% 1:10 37.5 900 4 3.2wt% 1:10 12 500 5 3.2wt% 1:10 12 700 6 3.2wt% 1:20 12 900
[0130] Comparative Example 1
[0131] This example adopts a method and process conditions similar to those of Example 1, except that the MoOx / C (type Z2) in step (1) is replaced with an equal mass of oxidized carbon powder prepared in Preparation Example 1; the specific steps are as follows:
[0132] (1) 12 mg of IrCl3·xH2O (metal source) and 109 mg of the oxidized carbon powder prepared in Preparation Example 1 were dispersed in 50 mL of water and subjected to ultrasonic treatment at 25°C and 40 kHz for 1 hour. The solvent was evaporated at 50°C using a rotary evaporator (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0133] (2) The intermediate obtained in step (1) is ground into an average particle size of 0.1 mm using a mortar, and then spread on a magnetic boat. The magnetic boat is placed in a quartz tube. In a nitrogen atmosphere, the temperature is increased to 900°C at a heating rate of 10°C / min and maintained at this condition for 1 h. The resulting sample is Ir / C.
[0134] Comparative Example 2
[0135] This embodiment adopts a method and process conditions similar to those of Embodiment 1, except that IrCl3·xH2O is not added in step (1); the specific steps are as follows:
[0136] (1) 109 mg of MoOx / C powder (type Z2) was dispersed in 50 mL of water and ultrasonically treated at 25°C and 40 kHz for 1 hour. The solvent was evaporated using a rotary evaporator at 50°C (time and pressure were the same as in Example 1), and the residue was collected and dried overnight.
[0137] (2) The intermediate obtained in step (1) is ground into an average particle size of 0.1 mm using a mortar, and then spread on a magnetic boat. The magnetic boat is placed in a quartz tube. In a nitrogen atmosphere, the temperature is increased to 900°C at a heating rate of 10°C / min and maintained at this condition for 1 h. The obtained sample is MO2C / C.
[0138] Test Case
[0139] Rotating disk electrode test method
[0140] 1. Take 1 mg of catalyst powder, 5 μL of 5 wt% Nafion solution (perfluorinated resin solution), add 895.5 μL of anhydrous ethanol and 99.5 μL of aqueous solution, and after ultrasonic dispersion, a uniformly dispersed catalyst ink can be obtained;
[0141] 2. Take 10 μL of the catalyst ink obtained in step 1 and apply it on the glassy carbon electrode twice. Use the rotating disk electrode method to test and keep the rotation speed at 1600 rpm. Test in a hydrogen-saturated 0.1 M KOH solution. Use linear voltammetry to collect the hydrogen oxidation polarization curve. Control the potential to scan from -0.2 V to 0.8 V, and the scan rate is 5 mV / s.
[0142] Membrane electrode preparation method:
[0143] 1. Weigh a certain amount of catalyst powder (control loading is 0.05 mg PGM / cm 2), dissolved in 1 mL of isopropanol and 50 uL of aqueous solution, added with 127 uL of 5% PAP-TP-100 ethanol solution of ionomer solution, strongly sonicated for 1 min and then sonicated in an ice bath for 2 h.
[0144] 2. Use commercially available Pt / C as the cathode catalyst, weigh 10 mg of Pt / C, dissolve the catalyst in 1 mL of isopropanol and 50 uL of aqueous solution, add 84 uL of 5% PAP-TP-100 ethanol solution, perform strong ultrasound for 1 min, and then place in an ice bath for 2 h.
[0145] 3. The catalyst ink dispersed by ultrasonic in the above steps 1 and 2 was sprayed symmetrically on both sides of the alkaline membrane (PAP-TP-85) successively. The anode loading measured by ICP was 0.05 mg. Ir / cm 2 , cathode loading is 0.4 mg Pt / cm 2 .
[0146] 4. Soak the alkaline membrane sprayed with the catalyst in a 3M NaOH solution overnight, then use ultrapure water to exchange the residual NaOH on the surface of the alkaline membrane, and gently absorb the moisture on the surface of the alkaline membrane with dust-free paper.
[0147] 5. Two gas diffusion layers (SGL 29BC) are sandwiched between the two sides of the alkaline membrane to form a membrane electrode (MEA), and the prepared membrane electrode is placed on a 5 cm 2 The membrane electrode is clamped in the graphite flow field plate with three snake flow channels.
[0148] Alkaline membrane fuel cell test method:
[0149] The battery fixture with MEA installed was heated to 95°C, hydrogen was introduced to the anode at a flow rate of 1000sccm, humidification temperature of 92°C, and back pressure of 200kPa; oxygen was introduced to the cathode at a flow rate of 500sccm, humidification temperature of 95°C, and back pressure of 250kPa. The polarization curve of the battery from open circuit voltage to 0.2V was recorded by linear voltammetry.
[0150] Potential stability test method:
[0151] Based on the rotating disk electrode test method, a constant potential (i.e., chronoamperometry) procedure was used to evaluate the electrochemical stability of the catalyst. The test was carried out in a H2-saturated 0.1 M KOH solution system at a constant potential of 50 mV, and the current loss ratio was calculated to evaluate the electrochemical stability of the catalyst.
[0152] Durability test method:
[0153] Based on the rotating disk electrode test method, a multi-cycle cyclic voltammetry program was used to perform an accelerated durability test of the catalyst. In a H2-saturated 0.1M KOH solution system, the potential window of 0-0.5V was scanned for several cycles at a scan rate of 0.1V / S, and the activity loss changes of the catalyst were analyzed to evaluate its durability.
[0154] The Ir / Mo2C / C composite material prepared by the present invention has excellent stability and alkaline hydrogen oxidation activity as an alkaline membrane fuel cell anode catalyst; in particular, the alkaline hydrogen oxidation activity, the peak power density and mass activity of the alkaline membrane fuel cell of Examples 1, 4 and 5 are better than those of Examples 2, 3 and 6.
[0155] The present invention provides the test data of Example 1, Example 3, Comparative Example 1, Comparative Example 2, Pt / C and PtRu / C as an example. It can be seen from the characterization that: Figure 1 TEM, XRD, HAADF-STEM and EDS mapping of M1 obtained in Example 1 of the present invention. Figure 1 In the figure, a and b represent TEM images of M1 obtained in Example 1 at different resolutions; c represents the XRD image of M1 obtained in Example 1; d represents the HAADF-STEM and EDS mapping image of M1 obtained in Example 1; it can be seen from the figure that the catalyst contains a Mo2C-modified carbon support at the atomic scale, and the Ir atoms are all single-atom dispersed on the carbon support.
[0156] Figure 2 The polarization curves of M1 obtained in Example 1, Pt / C (the aforementioned commercial product), PtRu / C (the aforementioned commercial product), Ir / C obtained in Comparative Example 1, and Mo2C / C obtained in Comparative Example 2 were tested in 0.1M KOH saturated with hydrogen. As can be seen from the figure, compared with Ir / C obtained in Comparative Example 1, Mo2C / C obtained in Comparative Example 2, Pt / C (the aforementioned commercial product) and PtRu / C (the aforementioned commercial product), M1 exhibits a higher HOR activity, and its anode current density increases sharply. At the same time, the Mo2C / C carrier has almost no HOR activity, indicating that the activity of the Ir / Mo2C / C composite material comes from the highly dispersed Ir active sites.
[0157] Figure 3 is based on Figure 2Comparison of the mass ratio exchange current and the activity of the corresponding metal nanoparticles calculated from the polarization curves of M1, Ir / C, Pt / C and PtRu / C. As can be seen from the figure, the activity of M1 is 12 times higher than that of Ir / C; the activity of M1 is 13 times higher than that of Pt / C; and the activity of M1 is 4.5 times higher than that of PtRu / C.
[0158] Figure 4 This is the performance diagram of the low anode catalyst loading alkaline membrane fuel cell assembled with M1 obtained in Example 1, Pt / C (the aforementioned commercial product), PtRu / C (the aforementioned commercial product), and Ir / C obtained in Comparative Example 1. As can be seen from the figure, when the anode loading is only 0.05 mg PGM / cm 2 In the case of M1, the alkaline membrane fuel cell has a thermal conductivity of 1.64 W / cm 2 The peak power density is higher than that of PtRu / C (0.91W / cm 2 )、Pt / C(0.51W / cm 2 ) and Ir / C(0.60W / cm 2 ).
[0159] Figure 5 yes Figure 4 The materials shown in the figure are used for fuel cell peak power density and mass activity diagram. For comparison, we normalize the PPD of MEA to the anode catalyst loading. As can be seen from the figure, the HEMFC (hydrogen oxygen fuel cell) assembled using M1 composite material has 32.8W / cm 2 Ir Ultra-high anode mass activity.
[0160] Figure 6 The chronoamperometric curves are obtained by testing M1 obtained in Example 1, Ir / C, Pt / C (the aforementioned commercial product), and PtRu / C (the aforementioned commercial product) obtained in Comparative Example 1 in 0.1M KOH saturated with hydrogen at a rotation speed of 900 rpm at a constant potential of 50 mV. The current density of M1 was maintained at 95% of the initial value after 120 hours of continuous operation, showing negligible attenuation. For Ir / C, Pt / C, and PtRu / C, after a short test of 20 hours, the current density was only maintained at 45%, 35%, and 33%, respectively. The decay rate of M1 is 0.042% per hour, which is much less than the decay rates of Ir / C (2.5% / h), Pt / C (2.9% / h), and PtRu / C (3.0% / h). It shows that the catalyst decay has slowed down by nearly two orders of magnitude.
[0161] Figure 7 yes Figure 6The constant potential test stability is shown in . It can be seen from the figure that the M1 obtained in Example 1 can operate stably under long-term test conditions. Compared with Ir / C, Pt / C (the aforementioned commercial products) and PtRu / C (the aforementioned commercial products) obtained in Comparative Example 1, the M1 obtained in Example 1 shows obvious stability advantages.
[0162] Figure 8 is M1 obtained in Example 1 (such as Figure 8 a in FIG), PtRu / C (the aforementioned commercial product) (as shown in FIG. Figure 8 b), Pt / C (the aforementioned commercial product) (as shown in Figure 8 c in the figure), the Ir / C obtained in the comparative example (as shown in Figure 8 The durability test was performed in the range of 0 to 0.5 V at 2 mV / s in 0.1 M KOH saturated with hydrogen (as shown in d). Figure 8 Figure a shows the polarization curves of M1 obtained in Example 1 before and after 10,000, 20,000 and 30,000 cycles of cyclic voltammetry testing. It can be seen from the figure that the polarization curves of the M1 composite material obtained in Example 1 completely overlap, that is, after 30,000 cycles of accelerated durability testing, the activity of the catalyst is completely unaffected and has extremely high stability. Figure 8 Figures b, c, and c show the polarization curves of PtRu / C, Pt / C, and Ir / C catalysts before and after 10,000 cycles of cyclic voltammetry test, respectively. It can be seen from the figure that the polarization curves before and after 10,000 cycles of cyclic voltammetry test of M1 have obvious attenuation.
[0163] Fig. 9 The accelerated durability test diagrams of M1 obtained in Example 1, Ir / C, Pt / C (the aforementioned commercial product), and PtRu / C (the aforementioned commercial product) obtained in Comparative Example 1 show that M1 obtained in Example 1 maintains its activity without any decrease during the entire ADT process, while PtRu / C, Pt / C, and Ir / C decayed by 65%, 76%, and 14% respectively in relative j0 (exchange current density) after scanning 10,000 cycles. This shows that M1 obtained in Example 1 has good stability and maintains its microstructure in the hydrogen oxidation reaction.
[0164] In order to make the description of this patent more concise, other non-core characterizations of the above-mentioned embodiments are not placed. These technical features are similar to the single-atom dispersion in the carbide carrier provided by the present invention to enhance the activity of alkaline hydrogen oxidation reaction and are similar to the Ir / Mo2C / C catalyst with the best performance, and should be considered to be within the scope of this patent specification.
[0165] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various specific technical features in any suitable manner. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. However, these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing an Ir / Mo2C / C composite material, characterized in that: include: (1) In the presence of water, a metal source and a carrier precursor are contacted and mixed and then evaporated to obtain an intermediate I; (2) heating the intermediate I under a protective atmosphere to obtain the Ir / Mo2C / C composite material; The metal source is a soluble compound capable of providing a metal active component, and the metal active component is Ir; Based on the total weight of the Ir / Mo2C / C composite material, the amount of the metal source is such that the loading amount of the metal active component is 1-15wt%; The elemental molar ratio of Ir to Mo in the Ir / Mo2C / C composite material is 1:5-15, and the metal active component is distributed on Mo2C in a single-atom dispersed state; The carrier precursor is MoO x / C composite, and the MoO x The / C composite is prepared by a preparation method comprising the following steps: (S1) dispersing carbon oxide powder, molybdenum pentachloride and a dispersant to obtain material A; (S2) in the presence of water, subjecting the material A to a heat-insulating reaction to obtain material B; (S3) freeze-drying the material B to obtain the MoO x / C complex.
2. The method according to claim 1, characterized in that In step (1), the metal source is IrCl3·xH2O and / or iridium acetylacetonate; And / or, in step (1), the conditions of the evaporation treatment include: temperature of 40-60°C, time of 0.5-1h, and pressure of -0.1Mpa to -0.05Mpa.
3. The method according to claim 1 or 2, characterized in that In step (2), the conditions of the heating treatment include: a temperature of 500-1000°C and a time of 0.5-1.5h; And / or, in step (2), before the heating treatment, the intermediate I is ground to an average particle size of 0.07-0.1 mm.
4. The method according to claim 1, characterized in that: In step (S1), the dispersant is selected from at least one of ethanol, isopropanol and methanol.
5. The method according to claim 1 or 4, characterized in that: In step (S2), the conditions for the heat preservation and heating reaction include: temperature of 80-100°C and time of 6-10h.
6. The method according to claim 1 or 4, characterized in that: The heat preservation and heating reaction is carried out under stirring conditions.