A iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer and its preparation method and application
By using iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer as a flame retardant in epoxy resin, the problems of easy combustion of polymer materials and pollution by bromine-containing flame retardants are solved. problem, achieving the efficient flame retardant effect and environmental friendliness of epoxy resin.
Patent Information
- Application Number
- CN202410268036.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-08
AI Technical Summary
Existing polymer materials such as epoxy resin are easy to burn at high temperatures and require a large amount of brominated flame retardants to achieve flame retardant effects. However, these flame retardants will produce harmful substances when burned at high temperatures, leading to environmental pollution and health risks. .
Using iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer as a flame retardant, green needle-like crystals were synthesized in a hydrothermal reaction with nickel salt and organic carboxylic acid. Modify epoxy resin to reduce the use of flame retardants and reduce environmental pollution.
This coordination polymer only needs a small amount of addition in epoxy resin to achieve a strong flame retardant effect. The iodine element decomposes during the combustion process to generate non-flammable gas, and the nickel element promotes the formation of carbon to form stable NiO, which significantly improves Improved flame retardant performance and environmental friendliness.
Smart Images

Figure CN118005946B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant materials, and in particular to an iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer and a preparation method and application thereof. Background Art
[0002] Polymer materials have been widely used in many fields such as electronic communications, biomedicine, aerospace, automotive industry, construction, etc. However, many polymer materials, such as epoxy resin, are highly flammable and easily decompose and burn at high temperatures, endangering human life and property safety. Flame retardants need to be added to them to make them flame retardant.
[0003] In order to make epoxy resin achieve the required flame retardant performance or grade, halogen-containing flame retardants are often used, such as decabromodiphenyl ether, tetrabromobisphenol A, tetrabromodipentaerythritol, brominated polystyrene, pentabromotoluene or hexabromocyclododecane and other bromine-containing flame retardants. Although these bromine-containing flame retardants have good flame retardancy, they usually require a large amount (the addition amount is usually more than 10%) to achieve a good flame retardant effect. Moreover, bromine-containing flame retardants will produce difficult-to-degrade harmful substances such as dioxin-like organic halogen chemicals when burned at high temperatures, which pollute the environment and affect human and animal health.
[0004] Therefore, how to reduce the usage of flame retardants and reduce environmental pollution is an urgent problem to be solved in this field. Summary of the invention
[0005] One of the purposes of the present invention is to provide a flame retardant polymer material which is environmentally friendly and has good flame retardancy.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: an iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer, the chemical formula of which is: [Ni2I(C7H5N4)2] n ; Crystallographic data: belongs to triclinic system, space group P-1, unit cell parameters: α=99.5890(10)°, β=109.0990(10)°, γ=105.2800(10)°, Dc=2.180g / cm 3 , Z=2, F(000)=522, final deviation factor R1=0.0237, wR2=0.0638.
[0007] Wherein, the crystal molecular structure of the above-mentioned coordination polymer is as follows:
[0008]
[0009] The second object of the present invention is to provide a method for preparing an iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer, which comprises the following steps:
[0010] Add appropriate amount of organic carboxylic acid, 3-(2-pyridyl)-1,2,4-triazole and nickel salt to a reaction container, add appropriate amount of water as solvent, stir for a period of time, add acid binding agent to adjust pH value, add ion regulator (for example, iodine-containing ion regulator, such as iodide), heat to 90-170°C, react for a period of time and cool to room temperature to obtain green needle-shaped crystals, which are the target product.
[0011] Preferably, the molar ratio of the organic carboxylic acid, 3-(2-pyridyl)-1,2,4-triazole and nickel salt is (1-6):(1-4):(1-3). For example, the amount of the organic carboxylic acid, 3-(2-pyridyl)-1,2,4-triazole and nickel salt used can be 1-6 mmol, 1-4 mmol, 1-3 mmol, respectively.
[0012] Preferably, the nickel salt is at least one of nickel chloride, nickel sulfate, nickel hydroxide, nickel acetate, nickel nitrate, nickel perchlorate, nickel fluoride, basic nickel carbonate, and nickel iodide.
[0013] Preferably, the acid binding agent is at least one of sodium hydroxide, potassium hydroxide, ammonia water, triethylamine and ethylenediamine.
[0014] Preferably, the pH value after adjustment by the acid binding agent is 4-9.
[0015] Preferably, the ion regulator is at least one of potassium iodide, sodium iodide and ammonium iodide.
[0016] Among them, the above-mentioned iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer can be used as a flame retardant.
[0017] In addition, the present invention also provides a flame retardant modified epoxy resin, wherein the iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer is added.
[0018] Preferably, the mass content of the iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer is 3% to 7% (preferably 5% to 7%).
[0019] The coordination polymer of the present invention contains halogen element iodine, which is an environmentally friendly halogen flame retardant element compared to bromine element which produces toxic gases during combustion. During combustion, iodine element is unstable and first decomposes to form HX. XO can capture H generated during combustion and absorb heat, effectively reducing the temperature of the local combustion center. At the same time, the triazole compound in the molecular structure belongs to an intumescent flame retardant and decomposes to generate NH3, N2, Nx O y , H2O and other non-combustible gases, dilute the concentration of combustible gas and oxygen, take away heat, and reduce the surface temperature of the polymer, both of which play a role in gas phase flame retardancy. In addition, the coordination polymer of the present invention contains transition metal element nickel, and the combustion process produces stable NiO compounds, which promote the formation of carbon and play a role in condensed phase flame retardancy. According to tests, the coordination polymer of the present invention has good flame retardancy when used as a flame retardant, and only a small amount of flame retardant needs to be added to make the epoxy resin achieve a strong flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the crystal molecular structure of iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer;
[0021] Figure 2 It is a one-dimensional chain diagram of iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer;
[0022] Figure 3 is a three-dimensional network diagram of iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer;
[0023] Figure 4 is the TG diagram of iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer;
[0024] Figure 5 The DSC graphs of blank epoxy resin and flame retardant modified epoxy resin. DETAILED DESCRIPTION
[0025] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with the examples, and the contents mentioned in the examples are not limitations of the present invention. It should be noted in advance that the following examples were completed in the laboratory, and those skilled in the art should understand that the amounts of the components given in the examples only represent the ratio relationship between the components, rather than specific limitations.
[0026] Example 1
[0027] 3mmol of organic carboxylic acid, 2mmol of 3-(2-pyridyl)-1,2,4-triazole and 2mmol of nickel salt (nickel sulfate is selected in this embodiment) are added to a 30mL hydrothermal reactor, a certain amount of water is added as a solvent, and the mixture is stirred in a greenhouse with a magnetic stirrer for 1 to 3 hours (2 hours in this embodiment), and an acid binding agent (potassium hydroxide is selected in this embodiment) is added to adjust the pH to 4 to 9 (pH to 7 in this embodiment); an ion regulator (sodium iodide is selected in this embodiment) is added, and then the reactor is heated to 90 to 170°C (130°C in this embodiment), reacted for 24 to 48 hours (36 hours in this embodiment), slowly cooled to room temperature by program temperature control, and a large amount of green needle-shaped crystals are obtained by opening the reactor to obtain an iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer.
[0028] Example 2
[0029] 1mmol of organic carboxylic acid, 1mmol of 3-(2-pyridyl)-1,2,4-triazole and 1mmol of nickel salt (nickel chloride is selected in this embodiment) are added to a 30mL hydrothermal reactor, a certain amount of water is added as a solvent, and the mixture is stirred in a greenhouse with a magnetic stirrer for 1 to 3 hours (1 hour in this embodiment), and an acid binding agent (sodium hydroxide is selected in this embodiment) is added to adjust the pH to 4 to 9 (pH = 4 in this embodiment); an ion regulator (potassium iodide is selected in this embodiment) is added, and then the reactor is heated to 90 to 170°C (90°C in this embodiment), reacted for 24 to 48 hours (24 hours in this embodiment), slowly cooled to room temperature by program temperature control, and a large amount of green needle-shaped crystals are obtained by opening the reactor to obtain an iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer.
[0030] Example 3
[0031] 6mmol of organic carboxylic acid, 4mmol of 3-(2-pyridyl)-1,2,4-triazole and 3mmol of nickel salt (nickel hydroxide is selected in this embodiment) are added to a 30mL hydrothermal reactor, a certain amount of water is added as a solvent, and the mixture is stirred in a greenhouse with a magnetic stirrer for 1 to 3 hours (3 hours in this embodiment), and an acid binding agent (ethylenediamine is selected in this embodiment) is added to adjust the pH to 4 to 9 (pH = 9 in this embodiment); an ion regulator (ammonium iodide is selected in this embodiment) is added, and then the reactor is heated to 90 to 170°C (170°C in this embodiment), reacted for 24 to 48 hours (48 hours in this embodiment), slowly cooled to room temperature by program temperature control, and a large amount of green needle-shaped crystals are obtained by opening the reactor to obtain an iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer.
[0032] The present invention also determines the crystal structure of the target product of Example 1, and the test results show that the organic carboxylic acid has no coordination, while the iodine atom participates in the coordination.
[0033] The chemical formula of the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer prepared in Example 1 is: [Ni2I(C7H5N4)2] n ; Crystallographic data: belongs to triclinic system, space group P-1, unit cell parameters: α=99.5890(10)°, β=109.0990(10)°, γ=105.2800(10)°, Dc=2.180g / cm 3 , Z=2, F(000)=522, final deviation factor R1=0.0237, wR2=0.0638.
[0034] The molecular structure of the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer prepared in Example 1 is shown in Figure 1 The main bond lengths and bond angles are listed in Table 1. Figure 1 It can be seen that each independent unit structure is composed of one iodine atom, two 3-(2-pyridyl)-1,2,4-triazole molecules and two nickel (II) ions. The two central atoms Ni(1) and Ni(2) are bridged by the 3-(2-pyridyl)-1,2,4-triazole anion, and the adjacent structural units are bridged by iodine atoms. The two nickel atoms [Ni(2), Ni(2 i )] and two iodine atoms [I(1),I(1 i )] form a parallelogram structure, two Ni(1) atoms [Ni(1),Ni(1 i )] are bridged by two 3-(2-pyridyl)-1,2,4-triazole anions to form a six-membered ring. The central atoms Ni(1) and Ni(2) are in a penta-coordinated and tetra-coordinated environment, respectively. In the structure with Ni(1) as the central atom, N(2), N(8), N(6), and N(5) are at the bottom of the pyramid, and the bond angles between the atoms on the plane are N(8 i )-Ni(1)-N(6)[95.65(10)°], N(5)-Ni(1)-N(6)[80.27(8)°], N(2)-Ni(1)-N(5)[92.27(8)°] and N(8 i )-Ni(1)-N(2)[92.10(11)°], with a total bond angle of 360.29° (close to 360°), indicating that N(2), N(8), N(6), and N(5) have good coplanarity. It also indicates that Ni is on the planes of N(2), N(8), N(6), and N(5), while N(1) is in the axial position. In the structure with Ni(2) as the central atom, each nickel atom is coordinated with two iodine atoms and two nitrogen atoms to form a four-coordinated deformed tetrahedral structure.
[0035] from Figure 2 It can be seen that the coordination polymer forms a one-dimensional chain polymer through the double bridge action of 3-(2-pyridyl)-1,2,4-triazole anion and iodine atom. Figure 3 It can be seen that the bridging 3-(2-pyridyl)-1,2,4-triazole anion extends into a spatial network structure, and the polymer formed by this structure has very good stability.
[0036] Table 1 Main bond lengths of coordination polymer materials Bond angle (°)
[0037]
[0038] Thermal stability test of iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer: The test results are as follows Figure 4 As can be seen from the figure, the whole decomposition process is divided into two stages. The first stage is the loss of one iodine atom, the temperature is 162 ~ 300 ℃, and the weight loss rate is about 24.0% (theoretical value: 23.74%); the second stage is the loss of two 3-(2-pyridyl)-1,2,4-triazole anions, the temperature is 300 ~ 475 ℃, and the weight loss rate is about 48.0% (theoretical value: 48.30%); because it is burned in an air atmosphere, the final NiO is about 28.0% (theoretical value: 27.96%). Since the complex forms a spatial network structure, it has good stability, which is reflected in the starting temperature of the thermal decomposition process being above 160 ℃.
[0039] The decomposition process is:
[0040]
[0041] Iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymers can be used in polymer flame retardancy, as follows:
[0042] Weigh 12g DDM in a 100mL beaker, heat to melt, cool to about 100°C, add iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer (mass content is 3%), stir and mix evenly, pour 30g epoxy resin weighed in advance and warmed in a 75°C oven into a beaker containing a curing agent (DDM) and a flame retardant (iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer), stir evenly and quickly cast into a 130*6.5*3 national standard oxygen index specimen and a 120*13*3.2 national standard vertical combustion specimen mold, cure at room temperature for 20h, then cure at 100°C for 3h, and then place in a 160°C vacuum drying oven for 1h, naturally cool to room temperature and demold to obtain a flame retardant modified epoxy resin sample to be tested.
[0043] Under the same conditions, two other flame retardant modified epoxy resin samples to be tested were prepared, and the only difference between the samples was the mass content of iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer, which were 5% and 7% respectively.
[0044] The blank (flame retardant-free) EP sample is numbered 1, and the EP samples containing flame retardants (iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer) are numbered 2-4 in sequence according to the flame retardant content.
[0045] Combustion performance test: The limiting oxygen index was measured with a JF3-oxygen index meter, and the UL-94 vertical combustion performance test was performed with a FZ-5401 vertical combustion instrument. The results are summarized in Table 2:
[0046] Table 2 LOI and UL-94 test results of flame retardant modified epoxy resin
[0047] Test No. Flame retardant weight / (w%) Limiting oxygen index LOI (%) UL-94 Flammability Rating 1 0 28.0 No level 2 3.0 34.0 VI, no dripping 3 5.0 36.2 V-0, no dripping 4 7.0 37.3 V-0, no dripping
[0048] a. Weight percentage refers to the total weight percentage of additives relative to (epoxy resin EP-51 + curing agent);
[0049] b. The determination of limiting oxygen index refers to the national standard method GB / T2406.2-2009, and the UL-94 vertical burning test adopts the GB / T 2408-2008 standard;
[0050] It can be seen from the above table that as the content of flame retardant in EP increases, the limiting oxygen concentration also increases. When the content reaches about 5%, its LOI value reaches 36.2%, and the UL-94 combustion grade reaches V-0. Compared with the blank EP (LOI: 28.0, T: 28s; does not extinguish when burning), the flame retardant effect is significantly enhanced.
[0051] Thermal stability test of flame retardant modified epoxy resin: DSC was used to analyze the heat absorption and release changes of blank and 5% content of coordination polymer flame retardant modified epoxy resin composite materials during the heating process, so as to calculate the glass transition temperature (Tg). Figure 5 As shown in the figure, the Tg of the EP blank epoxy resin composite material and the flame retardant epoxy resin composite material with 5% coordination polymer are 125.4℃ and 137.9℃ respectively. From this analysis, when the content of flame retardant added to the epoxy resin matrix is 5% while maintaining LOI and UL-94 reaching V-0 level, the thermal stability Tg of the composite material does not decrease, but increases, indicating that the polymer material generates new chemical bonds during the polymerization process.
[0052] In general, the present invention uses nickel salt, organic carboxylic acid and 3-(2-pyridyl)-1,2,4-triazole as raw materials to synthesize a transition metal nickel coordination polymer [Ni2I(C7H5N4)2] n (Its crystal molecular structure can be seen in Figure 1 ). The polymer has a certain thermal stability and does not decompose at a temperature of 160°C; it is applied to epoxy resin materials and has a good flame retardant effect. Its flame retardant mechanism is mainly reflected in two aspects. First, the polymer contains the halogen element iodine. Although it is currently less used due to its high price, it is an environmentally friendly halogen flame retardant element compared to the toxic gas produced during the combustion process of the bromine element. During the combustion process, the iodine element is unstable and first decomposes to form HX. XO can capture the H generated during the combustion process to absorb heat and effectively reduce the temperature of the local combustion center. At the same time, the triazole compound in the molecular structure is an intumescent flame retardant, which decomposes to produce NH3, N2, N x O y , H2O and other non-flammable gases dilute the concentration of flammable gases and oxygen, take away heat, and reduce the surface temperature of the polymer, both of which play a role in gas phase flame retardancy. Secondly, the polymer contains transition metal element nickel, and the combustion process produces stable NiO compounds, which promote the formation of carbon and play a role in condensed phase flame retardancy. The polymer synthesis process is simple, does not use organic solvents, is environmentally friendly, has a stable structure, good repeatability, and has a shorter crystal period than the solvent method and diffusion method. It is a flame retardant polymer material worthy of promotion.
[0053] In addition, it is worth mentioning that the present invention has the following advantages: (1) The coordination polymer is prepared by a hydrothermal reaction method using water as a solvent. No organic solvent is used in the synthesis process, and there is no organic solvent volatilization, which will not cause pollution to the environment. (2) The product is stable and has good repeatability. The crystal period obtained is shorter than that obtained by the solvent method and the diffusion method. (3) No decomposition is observed at a temperature of 160°C. The coordination polymer has a stable structure and is a polymer material with good thermal stability. (4) In addition, the polymer contains a large number of I atoms, which can form hydrogen bonds with the -OH of the epoxy resin during the polymerization process with the epoxy resin, thereby stabilizing the composite material. (5) The coordination polymer can be used as a flame retardant material in epoxy resin, and has a good flame retardant effect.
[0054] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present technical solution is within the protection scope of the present invention.
[0055] Finally, it should be emphasized that in order to allow ordinary technicians in the field to more easily understand the improvements of the present invention over the prior art, some descriptions of the present invention have been simplified, and for the sake of clarity, some other elements are omitted in this application document. Those skilled in the art should realize that these omitted elements may also constitute the content of the present invention.
Claims
1. An iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer, characterized in that: The chemical formula is: [Ni2I(C7H5N4)2] n ; Crystallographic data: belongs to triclinic system, space group P-1 , unit cell parameters: a =8.6380(9)Å, b =9.2434(9)Å, c =11.8588(12)Å, α =99.5890(10)º, β =109.0990(10)º, γ= 105.2800(10)°, V =829.25(15)Å 3 , Dc = 2.180g / cm 3 , Z =2, F (000) = 522, the final deviation factor R 1= 0.0237, wxya 2=0.0638.
2. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 1, characterized in that: The following steps are involved: Add appropriate amount of organic carboxylic acid, 3-(2-pyridyl)-1,2,4-triazole and nickel salt to a reaction container, add appropriate amount of water as solvent, stir for a period of time, add acid binding agent to adjust pH value, add iodine-containing ion regulator, heat to 90-170°C, react for a period of time and cool to room temperature to obtain green needle-shaped crystals, which are the target product.
3. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 2, characterized in that: The molar ratio of the organic carboxylic acid, 3-(2-pyridyl)-1,2,4-triazole and nickel salt is (1-6):(1-4):(1-3).
4. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 2, characterized in that: The nickel salt is at least one of nickel chloride, nickel sulfate, nickel hydroxide, nickel acetate, nickel nitrate, nickel perchlorate, nickel fluoride, basic nickel carbonate, and nickel iodide.
5. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 2, characterized in that: The acid binding agent is at least one of sodium hydroxide, potassium hydroxide, ammonia water, triethylamine and ethylenediamine.
6. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 2, characterized in that: The pH value after adjustment by the acid binding agent is 4-9.
7. The method for preparing the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 2, characterized in that: The ion regulator is at least one of potassium iodide, sodium iodide and ammonium iodide.
8. Use of the iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 1 as a flame retardant.
9. A flame retardant modified epoxy resin, characterized in that: The iodo-3-(2-pyridyl)-1,2,4-triazole coordination polymer according to claim 1 is added.
10. The flame retardant modified epoxy resin according to claim 9, characterized in that: The mass content of the iodinated 3-(2-pyridyl)-1,2,4-triazole coordination polymer is 3% to 7%.