A low-cost, high-toughness, ultra-high-strength steel and its preparation method

Through medium-carbon low-alloy design and micro-alloying element control, the microstructure of ultra-fine bainite, lath martensite, and film-like retained austenite is formed, which solves the problem of insufficient toughness and high cost of existing 2GPa-level ultra-high-strength steels. solve the problem and achieve high strength and high toughness under low alloy conditions to meet the application needs in the aerospace field.

CN118007027BActive Publication Date: 2024-10-18CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202311419753.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2024-10-18
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

The existing 2GPa ultra-high strength steel has insufficient toughness and high cost, making it difficult to meet the high requirements for material strength, toughness and uniformity in aerospace and other fields.

Method used

Using a medium-carbon low alloy design, a small amount of W, Mo and other micro-alloy elements are used to regulate the phase transformation behavior and control the generation of bainite. Combined with the precise control of the staged cooling rate and alloy composition, ultra-fine bainite and lath marten are formed. The microstructure of austenite and film-like retained austenite is optimized to improve the strength and toughness of the material by optimizing grain boundary treatment.

Benefits of technology

It achieves excellent strength and toughness under low alloy conditions, reduces the material cost of alloy elements, meets the demand for high-strength materials in aerospace and other fields, and significantly improves the strength and toughness of large structural parts with thick sections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118007027B_ABST
    Figure CN118007027B_ABST
Patent Text Reader

Abstract

The present invention relates to a low-cost, high-toughness ultra-high-strength steel and a preparation method thereof, which belongs to the technical field of ultra-high-strength alloy steel, and solves the problem that the existing ultra-high-strength steel has insufficient toughness and high cost. A low-cost, high-toughness ultra-high-strength steel, the weight percentage of its alloy components is: C: 0.38-0.42%, Mn: 1.20-1.70%, Si: 1.50-2.00%, Cr: 1.10-1.50%, Ni: 0.15-0.40%, Mo: 0.15-0.40%, W: 0.05-0.50%, Nb≤0.015%, B≤0.002%, the remainder is Fe and unavoidable impurities, and its microstructure is composed of ultrafine bainite, lath martensite, and film-like residual austenite; the preparation process includes smelting-soaking-forging or hot rolling-solid solution-tempering. The obtained low-cost, high-toughness ultra-high-strength steel has low cost and excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultra-high strength alloy steel, and in particular to a low-cost high-toughness ultra-high strength steel and a preparation method thereof. Background Art

[0002] Key components in aerospace and other fields have extremely high requirements for material performance, among which ultra-high strength and good toughness are crucial characteristics. Components in these fields often face harsh working environments and challenges, so materials need to have excellent mechanical properties.

[0003] At present, 2GPa-level ultra-high strength steel is a kind of material that has attracted much attention. Its application in aerospace and other engineering fields can significantly improve the safety level of materials and meet the requirements of some structural optimization at the same time. Traditional 2GPa-level ultra-high strength steel is usually based on tempered martensite matrix and is mainly divided into three categories: 1. Low-temperature tempering, ε-carbide-strengthened medium-carbon low-alloy series, such as 300M steel (40CrNi2Si2MoVA), which can reach a tensile strength of about 1920MPa and a hardness of about 82MPa·m 1 / 2 Fracture toughness; 2. Ultra-low carbon martensitic matrix, intermetallic compound strengthened martensitic aged steel, such as 18Ni series 350, 400 grades, although can achieve 2GPa level of strength, but the plastic toughness is significantly reduced; 3. Medium carbon high CoNi martensitic matrix, nano M2C carbide precipitation strengthened secondary hardening steel, represented by AerMet310 / 340, the maximum strength can reach 2.2GPa, but the plastic toughness is still insufficient.

[0004] The above three types of 2GPa-level high-strength steels all have high alloy material costs and manufacturing costs, which is a major constraint for application and promotion. At the same time, as the specifications of components increase, higher requirements are placed on the strength, toughness and uniformity of the materials. Therefore, there is an urgent need to develop a low-cost, low-alloy system of ultra-high-strength steel that meets the strength requirements of the 2GPa level, while having high toughness and achieving a low level in terms of alloy and manufacturing costs. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a low-cost, high-toughness ultra-high strength steel and a preparation method thereof, so as to solve at least one of the problems of insufficient toughness and high cost of existing 2GPa-level ultra-high strength steel.

[0006] On the one hand, the present invention provides a low-cost, high-toughness, ultra-high-strength steel, the alloy composition of which is calculated by weight percentage: C: 0.38-0.42%, Mn: 1.20-1.70%, Si: 1.50-2.00%, Cr: 1.10-1.50%, Ni: 0.15-0.40%, Mo: 0.15-0.40%, W: 0.05-0.50%, Nb≤0.015%, B≤0.002%, and the balance is Fe and unavoidable impurities.

[0007] Furthermore, the microstructure of the low-cost, high-toughness, ultra-high-strength steel consists of ultra-fine bainite, lath martensite, and film-like retained austenite.

[0008] Furthermore, in the microstructure, the volume ratio of ultrafine bainite, lath martensite and film-like retained austenite is 15-40:50-75:5-15.

[0009] Furthermore, in the microstructure, the spacing between the thin film retained austenite lamellae between the lath martensite is 100-200 nm; and the spacing between the thin film retained austenite lamellae between the ultrafine bainite is ≤100 nm.

[0010] On the other hand, the present invention also provides a method for preparing low-cost, high-toughness, ultra-high-strength steel, which is used to prepare the above-mentioned low-cost, high-toughness, ultra-high-strength steel, comprising the following steps:

[0011] Step S1: smelting, preparing alloy according to component content, and smelting to obtain steel ingot or steel billet;

[0012] Step S2: Soaking, placing the steel ingot or billet into a heating furnace for soaking treatment;

[0013] Step S3: forging or hot rolling, forging or hot rolling the steel ingot or steel billet after the soaking treatment to obtain a forging or rolled product;

[0014] Step S4: solution treatment, heating the forging or rolling piece for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process controls the cooling rate in stages;

[0015] Step S5: Tempering, subjecting the forged or rolled product after solution treatment to tempering treatment, and then air cooling or furnace cooling to room temperature.

[0016] Furthermore, in step S3, the initial forging or initial rolling temperature is 1150°C to 1220°C, and the final forging or final rolling temperature is 850°C to 900°C.

[0017] Furthermore, in step S4, the solution temperature is 900-980° C., and the holding time is 1-4 hours.

[0018] Furthermore, in step S4, the cooling process is controlled in stages to have a cooling rate of:

[0019] Solution temperature -800℃, cooling rate ≥0.5℃ / s;

[0020] 800℃-400℃, cooling rate ≥1℃ / s;

[0021] 400℃-300℃, cooling rate ≥0.2℃ / s;

[0022] 300℃-150℃, cooling rate ≥0.05℃ / s;

[0023] Air cool below 150℃ to room temperature.

[0024] Furthermore, in step S5, the tempering temperature is 200° C. to 300° C., and the tempering time is 2 to 10 hours.

[0025] Furthermore, an annealing process is also included between step S4 and step S5.

[0026] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0027] 1. The present invention adopts a medium-carbon low-alloy design, uses a small amount of micro-alloy elements such as W and Mo to regulate the phase transformation behavior, and in terms of preparation technology, controls the cooling rate in the medium and low temperature sections to control the effective generation of bainite, thereby obtaining a high-strength and toughness structure.

[0028] 2. The present invention purifies the austenite grain boundaries by adding alloying elements such as W and Mo to prevent the formation of coarse bainite and ferrite structures during the cooling process, and ensures the appropriate size of the austenite grains by setting an appropriate solid solution temperature, so that the bainite can effectively cut the grains. Through the above-mentioned precise control of the alloy composition and the optimization of the grain boundaries, excellent strength and toughness are achieved under low alloy conditions, meeting the application requirements of high-strength materials in the aerospace and other fields.

[0029] 3. The present invention controls the cooling process after solutionizing and controls the cooling rate in stages to ensure the moderate growth of ultrafine bainite, so as to obtain a microstructure composed of ultrafine bainite, lath martensite, and film-like residual austenite. The ultrafine bainite is used to cut the austenite grains, refine the microstructure, and effectively improve the strength and toughness of the material, so that the material has better comprehensive performance.

[0030] 4. In the low-cost, high-toughness, ultra-high-strength steel prepared by the present invention, the content of alloying elements such as nickel, chromium, molybdenum, etc. is precisely controlled at a low level, thereby reducing the material cost of the alloying elements. This optimization of the content of alloying elements balances the high toughness and manufacturing cost of the material, achieving dual considerations of performance and economy.

[0031] 5. Compared with the prior art, the present invention can significantly improve the toughness of large structural parts with thick sections. When processing large structural parts with thick sections, the prior art does not have a high internal cooling rate even if oil cooling is used. Without reasonable composition design, softening phases (such as bainite and ferrite) may appear in the material. If martensite is directly quenched, the martensite laths formed by shear are relatively coarse and the effect of cutting austenite grains is poor, and the material strength cannot reach 2GPa. The present invention uses ultrafine bainite cutting to cut large austenite grains into multiple small grains, thereby achieving material refinement and improving its strength and toughness.

[0032] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0034] Figure 1 is a microstructure morphology diagram of Example 1 of the present invention;

[0035] Figure 2 is a transmission image of ultrafine bainite / austenite of Example 1 of the present invention;

[0036] Figure 3 It is a microstructure morphology diagram of comparative example 2 of the present invention;

[0037] Reference numerals:

[0038] 1-Ultrafine bainite. DETAILED DESCRIPTION

[0039] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0040] A specific embodiment of the present invention discloses a low-cost, high-toughness, ultra-high-strength steel. The alloy components of the low-cost, high-toughness, ultra-high-strength steel are calculated by weight percentage as follows: C: 0.38-0.42%, Mn: 1.20-1.70%, Si: 1.50-2.00%, Cr: 1.10-1.50%, Ni: 0.15-0.40%, Mo: 0.15-0.40%, W: 0.05-0.50%, Nb≤0.015%, B≤0.002%, and the remainder is Fe and unavoidable impurities.

[0041] The reasons for limiting the composition of the ingot of the microalloyed high-toughness ultra-high strength steel and the method for producing the same in the present invention are explained below. The weight percentages in the composition are expressed only in %.

[0042] Carbon (C): Carbon is an important interstitial solid solution strengthening element, which can reduce the phase transition temperature of bainite and martensite. At the same time, carbon can also stabilize the presence of residual austenite. It should be noted that a higher carbon content may lead to a decrease in the toughness of the material and increase the risk of cracking during the cooling process. On the contrary, too low a carbon content may not fully exert the strengthening effect and may also produce low-strength phase transition products during the cooling process. Therefore, under the premise of ensuring the strength of the material, the toughness and preparation of the material should be ensured. In the present invention, the carbon content is controlled at 0.38-0.42%.

[0043] Manganese (Mn), chromium (Cr), nickel (Ni): The content of manganese, chromium and nickel in the alloy is critical for controlling the hardenability of the material and enhancing toughness. Manganese is a low-cost solid solution strengthening element that can improve the stability of austenite, but too high a manganese content may lead to element segregation. Therefore, while adding manganese to the alloy, it is also necessary to control the content of chromium and nickel. Chromium and nickel elements can not only enhance the toughness of the material, but also avoid cracking problems during the cooling process. It is worth noting that although nickel has excellent performance, its economy is poor. Taking all factors into consideration, in the present invention, the manganese content is controlled at 1.20-1.70%, the chromium content is controlled at 1.10-1.50%, and the nickel content is controlled at 0.15-0.40%.

[0044] Silicon (Si): The addition of silicon can inhibit the precipitation of cementite during cooling and tempering, improve tempering resistance, and expand the precipitation range of ε-carbide. This helps the material maintain a high strength without reducing toughness. In addition, silicon also plays an important role in the growth of bainite, promoting the formation of slender bainite and preventing the formation of short and thick bainite. However, too high a silicon content may increase the brittleness of the material and increase the difficulty of high-temperature oxidation and preparation. Therefore, in the present invention, the silicon content is controlled at 1.50-2.00%.

[0045] Molybdenum (Mo), tungsten (W): The addition of molybdenum and tungsten can play a role in solid solution strengthening and purify the austenite grain boundaries, thereby delaying the transformation of bainite. This can reduce the nucleation rate of bainite at the austenite grain boundaries, promote the segmentation of bainite, and improve the performance of the material. However, too much molybdenum may lead to the formation of coarse carbides, thereby reducing the economic efficiency of the material. Tungsten can improve the hydrogen embrittlement sensitivity of the material, but excessive addition may increase the risk of cracking. Therefore, in the present invention, the content of molybdenum is controlled at 0.15-0.4%, and the content of tungsten is controlled at 0.05-0.50%.

[0046] Niobium (Nb): Niobium is an important microalloying element that can achieve nano-precipitation strengthening. At the same time, niobium can also inhibit the coarsening of grains during austenitization and improve the performance consistency of the material. Therefore, in the present invention, the content of niobium should be controlled at ≤0.015%.

[0047] Boron (B): The addition of boron can prevent the premature formation of ferrite and bainite in the material, thereby preventing the deterioration of strength and toughness. In addition, boron can also improve the hardenability of the material and expand the cooling range of heat treatment. However, too much boron may affect the hot working performance of the material. Therefore, in the present invention, the content of boron is controlled to ≤0.002%.

[0048] Preferably, a low-cost, high-toughness, ultra-high-strength steel is provided, wherein the alloy components of the low-cost, high-toughness, ultra-high-strength steel are, by weight percentage, C: 0.39-0.41%, Mn: 1.23-1.38%, Si: 1.50-1.75%, Cr: 1.18-1.48%, Ni: 0.33-0.40%, Mo: 0.15-0.40%, W: 0.13-0.22%, Nb≤0.009%, B≤0.0005%, and the remainder is Fe and unavoidable impurities.

[0049] The specific embodiment of the present invention also discloses a method for preparing low-cost, high-toughness, ultra-high-strength steel, which is used to prepare the above-mentioned low-cost, high-toughness, ultra-high-strength steel, comprising the following steps:

[0050] Step S1: smelting, preparing alloy according to component content, and smelting to obtain steel ingot or steel billet;

[0051] Step S2: Soaking, placing the steel ingot or billet into a heating furnace for soaking treatment;

[0052] Step S3: forging or hot rolling, forging or hot rolling the steel ingot or steel billet after the soaking treatment to obtain a forging or rolled product;

[0053] Step S4: solution treatment, heating the forging or rolling piece for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process controls the cooling rate in stages;

[0054] Step S5: Tempering, subjecting the forged or rolled product after solution treatment to tempering treatment, and then air cooling or furnace cooling to room temperature.

[0055] Specifically, in step S2, the steel ingot or billet is placed in a heating furnace for soaking treatment at a soaking temperature of 1180-1250° C. for a soaking time of 1-5 hours. This step can eliminate fine inclusions in the matrix as much as possible, ensure uniform distribution of the structure, and alleviate macroscopic segregation of elements.

[0056] Specifically, in step S3, the initial forging or initial rolling temperature is 1150° C. to 1220° C., and the final forging or final rolling temperature is 800° C. to 900° C. In this step, the initial forging or initial rolling temperature is relatively high, which can increase the deformation amount of the alloy and reduce the deformation resistance of the alloy. The final rolling temperature of 800° C. to 900° C. can ensure that the hot deformed material is fully recrystallized and achieve grain refinement.

[0057] Specifically, in step S4, the solution temperature is 900-980°C and the holding time is 1-4 hours. In this temperature range, undissolved carbides can be effectively eliminated, while avoiding the problem of excessively large austenite grains due to excessively high temperatures, thereby achieving optimized treatment of grain boundaries. Preferably, the solution temperature is 935-950°C.

[0058] Specifically, in step S4, the cooling rate is controlled in stages as follows: during the cooling process, the solid solution temperature is 800°C, and the cooling rate is ≥0.5°C / s. Too slow cooling rate in the high temperature stage may cause inclusions such as carbides to re-precipitate and coarsen, affecting the toughness of the material; the cooling rate from 800°C to 400°C is ≥1°C / s to avoid ferrite phase transformation or a large amount of upper bainite formation, which reduces the strength of the material; the cooling rate from 400°C to 300°C is ≥0.2°C / s to further inhibit the formation of excessive bainite; the cooling rate from 300°C to 150°C is ≥0.05°C / s to avoid excessive residual austenite being retained and reducing the strength of the material; below 150°C is air cooling. During the cooling process, the total cooling time from 400°C to 150°C is not less than 250s to ensure the formation of a certain amount of bainite and form a cut to the original austenite.

[0059] Specifically, in step S5, the tempering temperature is 200°C to 300°C, and the tempering time is 2 to 10 hours. In this tempering temperature range, the formation of carbides can be effectively suppressed to avoid negative effects on toughness. At the same time, by suppressing the recovery of dislocations, the high strength of the matrix can still be maintained. Although the use of high Si content can also suppress the formation of carbides that are harmful to toughness, its cost is relatively high. Preferably, the tempering temperature is 220°C to 250°C, and the tempering time is 2 to 5 hours.

[0060] Preferably, between the forging or hot rolling and solutionizing steps, the forging or rolled piece is also annealed at a temperature of 500°C to 600°C for 3 to 5 hours. Annealing helps to form part of cementite or ferrite, softens the matrix, makes it easier to process and store, and avoids cracking or hydrogen embrittlement.

[0061] The present invention prepares low-cost, high-toughness and ultra-high-strength steel through precise design of alloy components, optimization of the preparation process and precise control of process parameters.

[0062] The present invention adjusts the carbon content to achieve the interstitial solid solution strengthening effect, reduces the bainite and martensite phase transition temperatures, is conducive to forming a fine bainite structure within a suitable temperature range, and improves the matching of strength and toughness. At the same time, the present invention fully considers the influence of the composition on the change of the grain boundary during the preparation process, optimizes the grain boundary during the preparation process, purifies the austenite grain boundary, inhibits the formation of coarse bainite, considers using low-temperature bainite to cut the austenite grains, and achieves a fine microstructure, thereby improving the strength and toughness of the material. Reduce the content of high-cost alloying elements such as nickel, molybdenum, and silicon, thereby reducing the manufacturing cost of the material, and at the same time, by accurately controlling the content, maintain its positive impact on the performance. The present invention comprehensively considers the interaction between various alloy elements to ensure that while optimizing a certain property, other properties will not be adversely affected; for example, the role of W and Mo elements is mainly to purify the grain boundary and inhibit the premature occurrence of bainite phase transformation, thereby preventing the formation of coarse bainite; Si element is conducive to the formation of bainite and ferrite, but the presence of W and Mo elements offsets this effect, and Si element can also promote the slender growth of bainite and prevent it from becoming wider, which makes bainite more likely to split austenite at the same bainite volume fraction, playing a significant role; C element and Mn, Cr, Ni elements have the effects of interstitial strengthening and solid solution strengthening respectively, and can also regulate the thermodynamic process of bainite phase transformation and the martensitic phase transformation point. On the basis of precise control of alloy composition, the present invention prepares low-cost, high-toughness ultra-high-strength steel through the preparation process of smelting-heat soaking-forging or hot rolling-solid solution-tempering and the control of process parameters, so that the material maintains ultra-high strength while significantly improving the toughness, and successfully reduces the manufacturing cost of the material, meeting the stringent application requirements of high-strength materials in fields such as aerospace, and achieving a dual balance of performance and economy.

[0063] The low-cost, high-toughness, ultra-high-strength steel prepared by the method of the present invention has a microstructure composed of ultra-fine bainite, lath martensite, and film-like retained austenite. Figure 1As shown, the ultrafine bainite divides the matrix, the lath martensite exists in the divided block, and the film retained austenite exists between the ultrafine bainite and the lath martensite, and mainly exists between the ultrafine bainite. The volume ratio of ultrafine bainite, lath martensite, and film-like retained austenite in the microstructure is 15-40:50-75:5-15. The interlamellar spacing of the film-like retained austenite between the lath martensite is 100-200nm, and the interlamellar spacing of the film-like retained austenite between the ultrafine bainite is ≤100nm.

[0064] The low-cost, high-toughness ultra-high-strength steel of the present invention has a tensile strength of ≥2GPa; a yield strength of ≥1500MPa; an elongation after fracture of ≥10%; a cross-sectional shrinkage of ≥36%; and a fracture toughness of ≥82MPa·m 1 / 2 .

[0065] Example 1

[0066] In this embodiment, the alloy composition is calculated by weight percentage as follows: C: 0.39%, Mn: 1.27%, Si: 1.50%, Cr: 1.18%, Ni: 0.40%, Mo: 0.40%, W: 0.22%, Nb: 0.009%, B: 0.0005%, and the balance is Fe and unavoidable impurities, which meets the alloy composition range required by the present invention.

[0067] The preparation process includes:

[0068] S1: smelting, preparing alloy according to component content, and smelting in a 200kg vacuum induction furnace to obtain steel ingots;

[0069] S2: Heat treatment: put the steel ingot into a heating furnace for heat treatment at a temperature of 1200°C and a time of 3 hours;

[0070] S3: Forging, forging the steel ingot after the soaking treatment, the initial forging temperature is 1150℃, the final forging temperature is 880℃, and the final cross-section is 60×60mm 2 Square forgings;

[0071] S4: annealing, cooling the square forging to room temperature, and then heating to 500°C for annealing, the annealing time is 3h;

[0072] S5: Solution treatment, heating the square forging for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process is controlled in stages to control the cooling rate;

[0073] Among them, the solution temperature is 950℃ and the holding time is 1h;

[0074] 950-800℃, cooling rate 2℃ / s;

[0075] 800-400℃, cooling rate 2℃ / s;

[0076] 400-300°C, cooling rate 1°C / s;

[0077] 300-150°C, cooling rate 0.5°C / s;

[0078] 150℃-room temperature, air cooling;

[0079] S6: Tempering: Temper the forging after solution treatment and then air cool it to room temperature.

[0080] Among them, the tempering temperature is 250℃ and the tempering time is 1h.

[0081] Example 2

[0082] The alloy composition of this embodiment is the same as that of embodiment 1, as shown in Table 1.

[0083] The preparation method of this embodiment is similar to that of Embodiment 1, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0084] Example 3

[0085] The alloy composition of this embodiment is the same as that of embodiment 1, as shown in Table 1.

[0086] The preparation method of this embodiment is similar to that of Embodiment 1, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0087] Example 4

[0088] The alloy composition of this embodiment is the same as that of embodiment 1, as shown in Table 1.

[0089] The preparation method of this embodiment is similar to that of Embodiment 1, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0090] Example 5

[0091] In this embodiment, the alloy composition is calculated by weight percentage as follows: C: 0.41%, Mn: 1.38%, Si: 1.64%, Cr: 1.40%, Ni: 0.33%, Mo: 0.16%, W: 0.17%, Nb: 0.008%, B: 0.0001%, and the balance is Fe and unavoidable impurities, which meets the alloy composition range required by the present invention.

[0092] The preparation process includes:

[0093] S1: smelting, preparing alloy according to component content, and smelting in a 200kg vacuum induction furnace to obtain steel ingots;

[0094] S2: Heat treatment: put the steel ingot into a heating furnace for heat treatment at a temperature of 1200°C and a time of 3 hours;

[0095] S3: rolling, rolling the steel ingot after the soaking treatment, with an initial rolling temperature of 1150°C and a final rolling temperature of 850°C, and finally obtaining a plate with a thickness of 60 mm;

[0096] S4: Annealing: air cool the plate to room temperature, then heat it to 600°C for annealing for 5 hours;

[0097] S5: Solution treatment, heating the plate for solution treatment, keeping warm, and then cooling to room temperature. The cooling process controls the cooling rate in stages;

[0098] Among them, the solution temperature is 950℃ and the holding time is 1h;

[0099] 950-800℃, cooling rate 2℃ / s;

[0100] 800-400℃, cooling rate 2℃ / s;

[0101] 400-300°C, cooling rate 1°C / s;

[0102] 300-150°C, cooling rate 0.5°C / s;

[0103] 150℃-room temperature, air cooling;

[0104] S6: Tempering: Temper the forging after solution treatment and then air cool it to room temperature.

[0105] Among them, the tempering temperature is 250℃ and the tempering time is 1h.

[0106] Example 6

[0107] The alloy composition of this embodiment is the same as that of embodiment 5, as shown in Table 1.

[0108] The preparation method of this embodiment is similar to that of Embodiment 5, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0109] Example 7

[0110] The alloy composition of this embodiment is the same as that of embodiment 5, as shown in Table 1.

[0111] The preparation method of this embodiment is similar to that of Embodiment 5, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0112] Example 8

[0113] The alloy composition of this embodiment is the same as that of embodiment 5, as shown in Table 1.

[0114] The preparation method of this embodiment is similar to that of Embodiment 5, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0115] Example 9

[0116] In this embodiment, the alloy composition is calculated by weight percentage as follows: C: 0.40%, Mn: 1.23%, Si: 1.75%, Cr: 1.48%, Ni: 0.38%, Mo: 0.15%, W: 0.13%, Nb: 0.002%, and the balance is Fe and unavoidable impurities, which meets the alloy composition range required by the present invention.

[0117] The preparation process includes:

[0118] S1: smelting, preparing alloy according to component content, and smelting in a 200kg vacuum induction furnace to obtain steel ingots;

[0119] S2: Heat treatment: put the steel ingot into a heating furnace for heat treatment at a temperature of 1200°C and a time of 2h.

[0120] S3: Forging, forging the steel ingot after the soaking treatment, the initial forging temperature is 1180℃, the final forging temperature is 900℃, and the final cross-section is 80×80mm 2 Square forgings;

[0121] S4: Annealing, cooling the square forging to room temperature, and then heating to 580°C for annealing, the annealing time is 3h;

[0122] S5: Solution treatment, heating the square forging for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process is controlled in stages to control the cooling rate;

[0123] Among them, the solution temperature is 950℃ and the holding time is 1h;

[0124] 950-800℃, cooling rate 2℃ / s;

[0125] 800-400℃, cooling rate 2℃ / s;

[0126] 400-300°C, cooling rate 1°C / s;

[0127] 300-150°C, cooling rate 0.5°C / s;

[0128] 150℃-room temperature, air cooling;

[0129] S6: Tempering: Temper the forging after solution treatment and then air cool it to room temperature.

[0130] Among them, the tempering temperature is 250℃ and the tempering time is 1h.

[0131] Example 10

[0132] The alloy composition of this embodiment is the same as that of embodiment 9, as shown in Table 1.

[0133] The preparation method of this embodiment is similar to that of Embodiment 9, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0134] Embodiment 11

[0135] The alloy composition of this embodiment is the same as that of embodiment 9, as shown in Table 1.

[0136] The preparation method of this embodiment is similar to that of Embodiment 9, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0137] Comparative Example 1

[0138] The alloy composition of this comparative example is the same as that of Example 1, as shown in Table 1.

[0139] The preparation method of this comparative example is similar to that of Example 1, except for the process parameters in the preparation process; some process parameters in the preparation process do not meet the requirements of the present invention, as shown in Table 2.

[0140] Comparative Example 2

[0141] The alloy composition of this comparative example is the same as that of Example 1, as shown in Table 1.

[0142] The preparation method of this comparative example is similar to that of Example 1, except that during the preparation process, water cooling is used for cooling after solid solution; as shown in Table 2.

[0143] Comparative Example 3

[0144] The alloy composition of this comparative example is the same as that of Example 5, as shown in Table 1.

[0145] The preparation method of this comparative example is similar to that of Example 5, except that during the preparation process, water cooling is used for cooling after solid solution; as shown in Table 2.

[0146] Comparative Example 4

[0147] The alloy composition of this comparative example is the same as that of Example 9, as shown in Table 1.

[0148] The preparation method of this comparative example is similar to that of Example 9, except for the process parameters in the preparation process; some process parameters in the preparation process do not meet the requirements of the present invention, as shown in Table 2.

[0149] Comparative Example 5

[0150] The alloy composition of this comparative example is the same as that of Example 9, as shown in Table 1.

[0151] The preparation method of this comparative example is similar to that of Example 9, except that during the preparation process, water cooling is used for cooling after solid solution; as shown in Table 2.

[0152] Comparative Example 6

[0153] In this comparative example, the alloy components are calculated by weight percentage: C: 0.42%, Mn: 1.10%, Si: 1.4%, Cr: 1.0%, Ni: 0.7%, Mo: 0.55%, W: 0.05%, Nb: 0.004%, B: 0.0002%, and the balance is Fe and unavoidable impurities, which does not meet the alloy composition range required by the present invention.

[0154] The preparation process includes:

[0155] S1: smelting, preparing alloy according to component content, and smelting in a 200kg vacuum induction furnace to obtain steel ingots;

[0156] S2: Heat treatment: put the steel ingot into a heating furnace for heat treatment at a temperature of 1180°C and a time of 3 hours;

[0157] S3: rolling, rolling the steel ingot after soaking treatment, with an initial rolling temperature of 1150°C and a final rolling temperature of 890°C, and finally obtaining a plate with a thickness of 80 mm;

[0158] S4: Annealing: air cool the plate to room temperature, then heat it to 600°C for annealing for 5 hours;

[0159] S5: Solution treatment, heating the plate for solution treatment, keeping warm, and then cooling to room temperature. The cooling process controls the cooling rate in stages;

[0160] Among them, the solution temperature is 950℃ and the holding time is 1h;

[0161] 950-800℃, cooling rate 2℃ / s;

[0162] 800-400℃, cooling rate 2℃ / s;

[0163] 400-300°C, cooling rate 1°C / s;

[0164] 300-150°C, cooling rate 0.5°C / s;

[0165] 150℃-room temperature, air cooling;

[0166] S6: Tempering: Temper the forging after solution treatment and then air cool it to room temperature.

[0167] Among them, the tempering temperature is 250℃ and the tempering time is 1h.

[0168] Comparative Example 7

[0169] The alloy composition of this comparative example is the same as that of comparative example 6, as shown in Table 1, and does not meet the alloy composition range required by the present invention.

[0170] The preparation method of this comparative example is similar to that of comparative example 6, except for the process parameters in the preparation process; the process parameters in the preparation process all meet the requirements of the present invention, as shown in Table 2.

[0171] Table 1 Alloy composition of examples and comparative examples (wt.%)

[0172]

[0173]

[0174] Table 2 Process parameters of the preparation process of the embodiments and comparative examples

[0175]

[0176]

[0177]

[0178] Table 3 Mechanical properties of the steels of the embodiments and comparative examples

[0179]

[0180]

[0181] Figure 1 The microstructure morphology of Example 1 is shown. As can be seen from the figure, the microstructure of the material is that ultrafine bainite penetrates the grains and divides the original austenite grains, and the rest is composed of lath martensite.

[0182] Figure 2 The ultrafine bainite / austenite transmission image of Example 1 is shown. It can be seen in the figure that the film-like residual austenite lamellae between the ultrafine bainite laths are at the level of 50nm. The ultrafine lamellae increase the stability of the thin film austenite, effectively increase the phase interface length, and effectively improve the strength and toughness of the structure.

[0183] Figure 3The microstructure morphology of comparative example 2 is shown. It can be seen from the figure that the microstructure matrix after water quenching is mainly martensite laths, and no ultrafine bainite is generated.

[0184] Forgings prepared in Examples 1-4 are made with the same alloy composition and different parameters in the preparation process, but all are within the range required by the present invention. The prepared forgings have excellent strength and toughness.

[0185] The plates prepared in Examples 5-8 use the same alloy composition and different parameters in the preparation process, but all are within the range required by the present invention. The prepared plates have excellent strength and toughness.

[0186] Forgings prepared in Examples 9-11 are made with the same alloy composition. Compared with Examples 1-4, the contents of Mo and W are relatively reduced, but still meet the requirements of the present invention. The parameters in the preparation process of Examples 9-11 are different, but all are within the range required by the present invention. Compared with Examples 1-4, the forgings finally prepared have slightly lower toughness but slightly improved strength, and still have excellent strength and toughness.

[0187] Comparative Example 1 uses the same alloy composition as Example 1 and meets the requirements of the present invention. However, the cooling rate in the cooling process after solutionization does not meet the requirements of the present invention, and the cooling is relatively slower. Although higher toughness is obtained, the strength is significantly reduced and does not reach the 2GPa level. This is mainly due to the low cooling rate in the medium temperature range, which leads to the formation of upper bainite / ferrite, softening of the material, and reduced strength.

[0188] Comparative Example 2 uses the same alloy composition as Example 1 and meets the requirements of the present invention. However, the cooling process after the solutionizing process does not control the cooling rate in stages, but is rapidly cooled by water cooling. The total cooling time from the solutionizing process to room temperature is less than 180 seconds, and the strength and toughness are significantly reduced, not reaching 2GPa, indicating that the matrix after the bainite segmentation is superior to the martensite matrix in terms of strength and toughness.

[0189] Comparative Example 3 uses the same alloy composition as Example 8 and meets the requirements of the present invention. However, the cooling rate is not controlled in stages during the cooling process after the solid solution, but it is rapidly cooled by water cooling. The total cooling time from the solid solution to the room temperature is less than 180s. Although the strength reaches 2GPa level, the toughness is obviously insufficient and does not meet the requirements of high-toughness ultra-high strength steel.

[0190] Comparative Example 4 uses the same alloy composition as Example 9 and meets the requirements of the present invention. However, the cooling rate in the cooling process after solutionization does not meet the requirements of the present invention, and the cooling is relatively slower. Although the toughness is improved, the tensile strength is significantly reduced, which is far from the 2 GPa level.

[0191] Comparative Example 5 uses the same alloy composition as Example 11 and meets the requirements of the present invention. However, the cooling rate is not controlled in stages during the cooling process after the solid solution, but it is rapidly cooled by water cooling. The total cooling time from the solid solution to room temperature is less than 180s, and its yield strength is slightly improved, but the tensile strength is reduced and does not reach 2GPa.

[0192] In the alloy composition of Comparative Example 6, the contents of Cr, Ni, Mn, Mo and Si elements do not meet the requirements of the present invention. Although the preparation process meets the requirements of the present invention, good toughness is still not achieved.

[0193] In the alloy composition of Comparative Example 7, the contents of Cr, Ni, Mn, Mo and Si elements do not meet the requirements of the present invention. Although the preparation process meets the requirements of the present invention, the strength of 2 GPa cannot be achieved.

[0194] The above description is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. The alloy design and preparation process of the present invention are also applicable to the production of large-scale high-toughness ultra-high strength steel. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A low-cost, high-toughness, ultra-high-strength steel, characterized in that: The alloy composition of the low-cost, high-toughness and ultra-high-strength steel is calculated by weight percentage as follows: C: 0.38-0.42%, Mn: 1.20-1.70%, Si: 1.50-2.00%, Cr: 1.10-1.50%, Ni: 0.15-0.40%, Mo: 0.15-0.40%, W: 0.05-0.50%, Nb: 0.002-0.015%, B≤0.002%, and the balance is Fe and unavoidable impurities; The microstructure of the low-cost, high-toughness and ultra-high-strength steel consists of ultra-fine bainite, lath martensite and film-like retained austenite; The low-cost, high-toughness and ultra-high-strength steel is prepared by the following steps: Step S1: smelting, preparing alloy according to component content, and smelting to obtain steel ingot or steel billet; Step S2: Soaking, placing the steel ingot or billet into a heating furnace for soaking treatment; Step S3: forging or hot rolling, forging or hot rolling the steel ingot or steel billet after the soaking treatment to obtain a forging or rolled product; Step S4: solution treatment, heating the forging or rolling piece for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process controls the cooling rate in stages; Step S5: tempering, subjecting the forged or rolled product after solid solution treatment to tempering, and then air cooling or furnace cooling to room temperature; In the step S3, the initial forging or initial rolling temperature is 1150°C to 1220°C, and the final forging or final rolling temperature is 850°C to 900°C; In step S4, the solution temperature is 900-980°C and the holding time is 1-4h; In the step S4, The cooling process is divided into stages to control the cooling rate: Solution temperature -800℃, cooling rate ≥0.5℃ / s; 800℃-400℃, cooling rate ≥1℃ / s; 400℃-300℃, cooling rate ≥0.2℃ / s; 300℃-150℃, cooling rate ≥0.05℃ / s; Air cool below 150℃ to room temperature; During the cooling process, the total cooling time from 400° C. to 150° C. is not less than 250 seconds.

2. The low-cost, high-toughness, ultra-high-strength steel according to claim 1, characterized in that: In the microstructure, the volume ratio of ultrafine bainite, lath martensite and film-like retained austenite is 15-40:50-75:5-15.

3. The low-cost, high-toughness, ultra-high-strength steel according to claim 2, characterized in that: In the microstructure, the spacing between the film-like retained austenite lamellae between the lath martensite is 100-200nm; the spacing between the film-like retained austenite lamellae between the ultrafine bainite is ≤100nm.

4. A method for preparing low-cost, high-toughness, ultra-high-strength steel, characterized in that: The method for preparing the low-cost, high-toughness and ultra-high-strength steel according to any one of claims 1 to 3 comprises the following steps: Step S1: smelting, preparing alloy according to component content, and smelting to obtain steel ingot or steel billet; Step S2: Soaking, placing the steel ingot or billet into a heating furnace for soaking treatment; Step S3: forging or hot rolling, forging or hot rolling the steel ingot or steel billet after the soaking treatment to obtain a forging or rolled product; Step S4: solution treatment, heating the forging or rolling piece for solution treatment, keeping the temperature, and then cooling to room temperature. The cooling process controls the cooling rate in stages; Step S5: tempering, subjecting the forged or rolled product after solid solution treatment to tempering, and then air cooling or furnace cooling to room temperature; In the step S3, the initial forging or initial rolling temperature is 1150°C to 1220°C, and the final forging or final rolling temperature is 850°C to 900°C; In step S4, the solution temperature is 900-980°C and the holding time is 1-4h; In the step S4, The cooling process is divided into stages to control the cooling rate: Solution temperature -800℃, cooling rate ≥0.5℃ / s; 800℃-400℃, cooling rate ≥1℃ / s; 400℃-300℃, cooling rate ≥0.2℃ / s; 300℃-150℃, cooling rate ≥0.05℃ / s; Air cool below 150℃ to room temperature; During the cooling process, the total cooling time from 400° C. to 150° C. is not less than 250 seconds.

5. The preparation method according to claim 4, characterized in that: In the step S4, the solution temperature is 930-980° C., and the holding time is 1-2 hours.

6. The preparation method according to claim 5, characterized in that: In the step S5, the tempering temperature is 200° C. to 300° C., and the tempering time is 2 to 10 hours.

7. The preparation method according to claim 4, characterized in that: Annealing treatment is also included between step S4 and step S5.

Citation Information

Patent Citations

  • A High-toughness Wear-resistant Steel and Its Manufacturing Method Used for Cold Environment and Heavy Load Railway Frogs

    AU2020101312A4

  • METHOD FOR MANUFACTURING A STEEL PART AND HOT-ROLLED STEEL PART

    BR112019024416A2

  • Bainite-martensite-austenite multi-phase wear-resistant steel plate and manufacturing method thereof

    CN104451436A

  • High-toughness ultrahigh-strength steel and manufacturing method thereof

    CN114107821A

  • High-hardness wear-resistant steel with excellent low-temperature impact toughness and manufacturing method thereof

    CN114729435A