A composite fiber modified SMA asphalt mixture and preparation method thereof
Through the combination of modified basalt fiber and glass fiber and co-solvent compounding technology, a composite fiber cross-linked network is formed, which solves the problem of insufficient performance of existing asphalt mixtures in complex environments and significantly improves rutting resistance, shear resistance and Freeze-thaw resistance.
Patent Information
- Application Number
- CN202410348389.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing asphalt mixtures have insufficient rutting resistance, shear strength, water damage resistance and freeze-thaw resistance in high-temperature, heavy-load, rainy and cold areas, making it difficult to meet the requirements for use in complex environments.
Composite fiber-modified SMA asphalt mixture is used to form composite fibers through the combination of modified basalt fiber and glass fiber, and the melting and mixing of SMA asphalt and rubber powder is promoted through the compound external admixture of cosolvent and solubilizer to form The three-dimensional network cross-linked with composite fibers improves deformation resistance and freeze-thaw resistance.
Significantly improves the rutting resistance, shear strength and freeze-thaw resistance of asphalt mixtures, reduces the erosion of water on the mixture, enhances compactness and adhesion, prevents moisture from forming voids and cracks, and improves water damage resistance.
Smart Images

Figure BDA0004759121910000021 
Figure BDA0004759121910000031 
Figure BDA0004759121910000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt mixture processing, and in particular to a composite fiber modified SMA asphalt mixture and a preparation method thereof. Background Art
[0002] Asphalt mixture is an important material for road construction, and its performance directly affects the service life of the road surface and driving safety. In recent years, with the continuous increase in traffic volume and the increasing axle load of vehicles, higher requirements have been placed on the performance of asphalt mixture. Especially in high temperature, heavy load, rainy and cold areas, the anti-rutting ability, shear strength, water damage resistance and freeze-thaw resistance of asphalt mixture have become the focus of attention.
[0003] Asphalt mixtures in the prior art mainly improve their performance by adjusting the ratio of asphalt and aggregate, but this method often has limitations and is difficult to meet complex and changing environmental and usage requirements. High-strength hydrophobic fiber materials, such as polypropylene fibers or glass fibers, are added to asphalt mixtures to enhance the bearing capacity, water damage resistance, shear strength and freeze-thaw resistance of asphalt mixtures. However, there are significant differences in the chemical properties of inorganic fiber materials and asphalt. This difference in chemical properties may make it difficult for the two to form stable chemical bonds or physical adsorption at the interface, reducing their compatibility, resulting in the bearing capacity, shear strength, water damage resistance and freeze-thaw resistance of asphalt mixtures need to be further improved.
[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a composite fiber modified SMA asphalt mixture and a preparation method thereof, so as to solve the technical problem that the bearing capacity, shear strength, water damage resistance and freeze-thaw resistance of asphalt mixture in the prior art need to be further improved.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A composite fiber modified SMA asphalt mixture, comprising the following components in parts by weight: 50-60 parts of composite fiber, 500-600 parts of aggregate, 25-35 parts of admixture, 250-350 parts of SMA asphalt and 50-80 parts of rubber powder;
[0008] The composite fiber is composed of modified basalt fiber and modified glass fiber in a weight ratio of 5:3.
[0009] Furthermore, the aggregate is composed of coarse aggregate, fine aggregate and mineral powder in a weight ratio of 5:2:1, the particle size of the coarse aggregate is 10-20 mm, and the particle size of the fine aggregate is 2-8 mm; the mineral powder is limestone powder with a particle size less than 2 mm; the admixture is composed of a cosolvent and a solubilizer in a weight ratio of 5:3, the cosolvent is dibutyl phthalate, and the compatibilizer is composed of 120# solvent oil and kerosene in a weight ratio of 1:3; the rubber powder is composed of styrene-butadiene rubber and natural rubber in a weight ratio of 1:1.
[0010] Further, the modified glass fiber is processed by the following steps:
[0011] A1. Sodium lignin sulfonate, 1,4-butanediol and chloroform are added to a nitrogen-protected reactor and stirred until the system is dissolved. A catalyst is added to the reactor. The temperature of the reactor is raised to reflux. A 4,4'-oxydiphthalic anhydride solution is added dropwise to the reactor. After the addition is complete, the reaction is carried out at a temperature of 6-7 hours. A capping agent is added to the reactor. The reaction is carried out at a temperature of 4-6 hours. The modified sodium lignin sulfonate is obtained by post-treatment.
[0012] The synthetic reaction equation of modified sodium lignin sulfonate includes:
[0013]
[0014]
[0015] Where:
[0016] R1:
[0017] R2:
[0018] Sodium lignin sulfonate, 1,4-butanediol and 4,4'-oxydiphthalic anhydride are used as raw materials and an esterification reaction is carried out under the condition of a catalyst to generate a polyester with a long straight-chain structure terminated by sodium lignin sulfonate and phthalic anhydride. The amino group modified on the surface of the end-capping agent can undergo an amidation reaction with diphthalic anhydride to form sodium lignin sulfonate and a modified sodium lignin sulfonate with a long straight-chain structure terminated by the end-capping agent.
[0019] A2, adding modified sodium lignin sulfonate and chloroform into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 50-55°C, adding isocyanatepropyltriethoxysilane dropwise into the reactor, and after the addition is complete, heat-retaining the reaction for 3-5 hours, and post-processing to obtain a modifier;
[0020] The carboxyl group on the modified sodium lignin sulfonate undergoes a condensation reaction with the isocyanate group on the isocyanatepropyltriethoxysilane to form a modifier having a siloxane bond-modified modified sodium lignin sulfonate.
[0021] A3, adding chopped glass fiber and activation solution into the reactor and stirring, raising the temperature of the reactor to 70-80°C, keeping the temperature for 2-3h, and post-treating to obtain pre-treated glass fiber;
[0022] The chopped glass fibers are treated with an activation liquid for heat preservation. The activation liquid can react with the surface of the glass fibers, remove impurities on the fiber surface, cause silicates to dissolve or rearrange, and increase the roughness and surface activity of the glass fiber surface.
[0023] A4. Add pre-treated glass fiber, anhydrous ethanol, purified water and sodium hydroxide into a reactor and stir. Raise the temperature of the reactor to 65-75°C. Add modifiers into the reactor in batches. Keep the temperature for 4-5 hours and post-treat to obtain modified glass fiber.
[0024] The siloxane bonds on the modifier are hydrolyzed in an alkaline environment and react with the surface active groups of the pre-treated glass fiber to form a graft modification on the surface of the pre-treated glass fiber.
[0025] Furthermore, in step A1, the amount ratio of sodium lignin sulfonate, 1,4-butanediol, and 4,4'-oxydiphthalic anhydride is 1 mol: 3 mol: 3.2 mol, the 4,4'-oxydiphthalic anhydride solution is composed of 4,4'-oxydiphthalic anhydride and chloroform in a weight ratio of 1:3, the amount ratio of sodium lignin sulfonate, chloroform, catalyst and end-capping agent is 2g: 7mL: 0.5g: 4g, and the catalyst is N-methylmorpholine; the post-treatment operation in step A1 includes: after the reaction is completed, the reactor is kept warm, and the solvent is evaporated under reduced pressure to obtain modified sodium lignin sulfonate; in step A2, the amount ratio of modified sodium lignin sulfonate, chloroform and isocyanatepropyltriethoxysilane is 4g: 15mL: 2g; the post-treatment operation in step A2 includes: after the reaction is completed, the reactor is kept warm at 50-55° C., and the solvent is evaporated under reduced pressure, The modifier is obtained; in step A3, the length of the chopped glass fiber is 20-25 mm, the activation solution is a 10 wt% sodium hydroxide solution, and the amount ratio of the chopped glass fiber to the activation solution is 1 g: 10 mL; the post-processing operation in step A3 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed with purified water until it is neutral, and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80° C. and dried to constant weight to obtain pre-treated glass fiber; in step A4, the amount ratio of the pre-treated glass fiber, anhydrous ethanol, purified water, sodium hydroxide and the modifier is 3 g: 18 mL: 6 mL: 1 g: 4 g, and the post-processing operation in step A4 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed with anhydrous ethanol twice, and then dispersed in ether, and stirred and dispersed for 40 minutes to obtain modified glass fiber.
[0026] Furthermore, the preparation method of the capping agent is: adding nano iron oxide and dispersion into a reactor and stirring, raising the temperature of the reactor to 65-75°C, adding 3-aminopropyltriethoxysilane into the reactor, keeping the temperature for 6-8h, and post-treating to obtain the capping agent.
[0027] In the dispersion environment, while 3-aminopropyltriethoxysilane and nano-iron oxide are uniformly dispersed, the siloxane bonds on 3-aminopropyltriethoxysilane are hydrolyzed and react with the surface active groups of the nano-iron oxide to generate a capping agent with 3-aminopropyltriethoxysilane-coated modified nano-iron oxide.
[0028] Furthermore, the dosage ratio of the nano iron oxide, the dispersion and 3-aminopropyltriethoxysilane is 3g:10mL:2g, the dispersion is composed of 70vt% ethanol, sodium hydroxide, sodium dodecyl sulfate and secondary alcohol polyoxyethylene ether in a dosage ratio of 100mL:7g:2g:1g, and the post-treatment operation includes: after the reaction is completed, filtering, washing the filter cake with purified water for 5 times and then with anhydrous ethanol for 2 times, transferring the filter cake to a drying oven at a temperature of 55-65°C, and vacuum drying to constant weight to obtain a capping agent.
[0029] Further, the modified basalt fiber is processed by the following steps:
[0030] B1. Put the basalt fiber into a muffle furnace, raise the temperature of the muffle furnace to 480-520°C, keep it warm for 3-4 hours, and naturally cool it down to room temperature to obtain heat-treated fiber;
[0031] B2, adding the heat-treated fiber and the pretreatment solution into a reactor and stirring, raising the temperature of the reactor to 65-75°C, keeping the temperature for 4-6 hours, and post-treating to obtain the pretreated fiber;
[0032] B3. Add the pretreated fiber, anhydrous ethanol, purified water and hydrochloric acid into the reactor and stir. The temperature of the reactor is increased to 60-70°C. Triethoxy[4-(2-oxirane-1)butyl]silane is added into the reactor. The reaction is kept warm for 2-3 hours. The modified basalt fiber is obtained by post-treatment.
[0033] The synthetic reaction principle of modified basalt fiber is:
[0034]
[0035] Using triethoxy[4-(oxiran-2-yl)butyl]silane as the modification molecule, under acidic conditions, the siloxane bonds on triethoxy[4-(oxiran-2-yl)butyl]silane are hydrolyzed to form silanol groups, which then react with the active groups on the surface of the pretreated fiber to form surface modification on the basalt fiber surface.
[0036] Furthermore, in step B1, the length of the basalt fiber is 10-25 mm; in step B2, the pretreatment solution is composed of 6 mol / L sulfuric acid, 3 mol / L nitric acid and octadecyltrimethylammonium bromide in a dosage ratio of 30 mL: 50 mL: 4 g; the post-treatment operation in step B2 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, standing for 20-30 minutes, skimming the upper suspension, washing the lower solid with purified water 5 times, draining, and transferring the filter cake to a drying oven at a temperature of 70-80 ° C, and drying to constant weight to obtain to pretreated fiber; in step B3, the amount ratio of pretreated fiber, anhydrous ethanol, purified water, hydrochloric acid and triethoxy [4- (oxiran-2-yl) butyl] silane is 3g: 10mL: 3mL: 2mL: 2g, and the concentration of hydrochloric acid is 6-8mol / L; the post-treatment operation in step B3 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with purified water to neutrality, the filter cake is transferred to a drying oven at a temperature of 60-70°C, and vacuum dried to constant weight to obtain modified basalt fiber.
[0037] A method for preparing a composite fiber modified SMA asphalt mixture comprises the following steps:
[0038] S1. Add composite fiber and aggregate into a mixer and stir for 2-3 minutes to obtain a premix;
[0039] S2. Add SMA asphalt, admixtures and rubber powder into a mixer, increase the mixer temperature to 150-180°C, and pre-mix for 30-50 minutes to obtain primary mixed asphalt;
[0040] S3. The temperature of the premix is raised to 150-180°C. Under stirring, the primary mixed asphalt is slowly added to the premix, stirred for 45-60 minutes under heat preservation, and then transferred to a heat preservation box at a temperature of 150-180°C to obtain an asphalt mixture.
[0041] The present invention has the following beneficial effects:
[0042] 1. When preparing the asphalt mixture of the present invention, modified glass fiber and modified basalt fiber are combined to form composite fibers, and the composite fibers are mixed with aggregates to form a premix. Through experimental exploration, an admixture composed of a cosolvent and a bulking agent is obtained, and under the action of the admixture, SMA asphalt and rubber powder are promoted to melt and mix under high temperature to form a uniform primary mixed asphalt with a fluid state. The primary mixed asphalt and the premix are then mixed under a high temperature environment to form a three-dimensional network cross-linked by the composite fibers, thereby improving the deformation resistance of the asphalt mixture under dynamic loads and its ability to maintain shape stability when subjected to external forces, reducing the erosion of moisture on the asphalt mixture, improving its stability in a water environment, reducing the stress concentration phenomenon caused by moisture during freezing and melting, and improving its freeze-thaw resistance.
[0043] 2. When preparing the asphalt mixture of the present invention, the surface of the activated glass fiber is modified by a modifier to prepare a modified sodium lignin sulfonate-coated modified glass fiber with a long straight chain structure terminated by sodium lignin sulfonate and nano-iron oxide, and the pretreated fiber is surface-modified with triethoxy [4-(oxirane-2-yl) butyl] silane after heat treatment in sequence to form a modified basalt fiber with an oxirane group modified on the surface. Oxidation is an organic compound with a three-membered ring structure in which the oxygen atom has a strong reactivity. Under high temperature conditions, the epoxy oxygen atom of oxirane is It may be more susceptible to electrophilic attack by carbonyl carbon in carboxyl group to produce nucleophilic substitution reaction and form chemical crosslinking. By controlling the specifications of glass fiber and basalt fiber, the modified glass fiber and modified basalt fiber form three-dimensional network crosslinking bonded by chemical bonds in asphalt mixture, which can improve the shear strength, rutting resistance and freeze-thaw resistance of asphalt concrete. The water absorption of modified glass fiber and modified basalt fiber is weak. The synergy between the two can reduce the erosion and damage of water to asphalt concrete. The fiber can also improve the density and adhesion of asphalt concrete, prevent water from forming voids and cracks inside the asphalt concrete, thereby further improving its resistance to water damage.
[0044] 3. When preparing the asphalt mixture of the present invention, the glass fiber is subjected to alkali treatment, and the concentration of the activation solution is explored. While obtaining pre-treated glass fiber with high surface activity, the structural damage to the glass fiber caused by the alkali treatment is reduced, so that the modification can evenly coat the pre-treated glass fiber. Nano-iron oxide has a small size effect and a high specific surface area at the nanoscale, thereby effectively improving the interfacial properties between the glass fiber and asphalt. Sodium lignin sulfonate is a natural polymer compound with good dispersibility. It reduces the agglomeration of fibers in asphalt and promotes the uniform dispersion of fibers in SMA asphalt mixtures. The dispersibility and compatibility improvement of sodium lignin sulfonate can provide favorable conditions for the uniform distribution of nano-iron oxide on the fiber surface. The reinforcing effect of nano-iron oxide can further enhance the adhesion and overall performance between the fiber and asphalt, so that the glass fiber can be evenly dispersed in the asphalt mixture. After the basalt fiber is subjected to high-temperature treatment, it is pre-treated with a pretreatment solution to promote the surface of the basalt fiber. After the impurities and residues are carbonized, the basalt fiber is treated with a pretreatment solution to make its surface cleaner and smoother, while increasing the active sites on the surface of the basalt fiber, providing more binding points for subsequent surface modification. The pretreated fiber is surface-modified with triethoxy[4-(2-oxirane-1)butyl]silane to form a modified basalt fiber modified with oxirane groups. The oxirane groups have good reactivity and compatibility, and can interact with the active components in asphalt. This interaction enhances the adhesion between the fiber and asphalt, making the fiber easier to disperse evenly in the asphalt mixture. DETAILED DESCRIPTION
[0045] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Example 1
[0047] This embodiment provides a method for preparing a composite fiber modified SMA asphalt mixture, comprising the following steps:
[0048] S1. Preparation of modifier
[0049] 70vt% ethanol, sodium hydroxide, sodium dodecyl sulfate and secondary alcohol polyoxyethylene ether were mixed uniformly in a dosage ratio of 100mL:7g:2g:1g to obtain a dispersion for later use;
[0050] Weigh: 12 g of nano iron oxide and 40 mL of dispersion liquid are added to a reactor and stirred. The temperature of the reactor is raised to 65°C. 8 g of 3-aminopropyltriethoxysilane is added to the reactor. The reaction is kept warm for 6 hours. The temperature of the reactor is lowered to room temperature. The filter is filtered and the filter cake is washed with purified water 5 times and then with anhydrous ethanol 2 times. The filter cake is transferred to a drying oven at a temperature of 55°C and vacuum dried to constant weight to obtain a capping agent.
[0051] Weigh: 53.5 g of sodium lignin sulfonate, 27.0 g of 1,4-butanediol, and 187.3 mL of chloroform, add to a nitrogen-protected reactor and stir until the system is dissolved, add 13.4 g of N-methylmorpholine to the reactor, raise the temperature of the reactor to reflux the system, dropwise add 397.1 g of 4,4'-oxydiphthalic anhydride solution to the reactor, and keep the temperature for 6 h. Add 107 g of a capping agent to the reactor, keep the temperature for 4 h, keep the reactor warm and evaporate the solvent under reduced pressure to obtain modified sodium lignin sulfonate;
[0052] Weigh: 100 g of modified sodium lignin sulfonate and 375 mL of chloroform are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 50°C. 50 g of isocyanatepropyltriethoxysilane is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 3 hours. The reactor is kept warm at 50°C, and the solvent is evaporated under reduced pressure to obtain a modifier.
[0053] S2. Preparation of modified glass fiber
[0054] Weigh: 20 g of chopped glass fiber with a length of 20-25 mm and 200 mL of 10 wt% sodium hydroxide solution, add them into a reactor and stir, raise the temperature of the reactor to 70° C., keep warm for 2 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, drain, transfer the filter cake to a drying oven at a temperature of 70° C., and dry to constant weight to obtain pre-treated glass fiber;
[0055] Weigh: 15 g of pretreated glass fiber, 90 mL of anhydrous ethanol, 30 mL of purified water and 5 g of sodium hydroxide, add them into a reactor and stir, raise the temperature of the reactor to 65°C, divide 20 g of the modifier into 5 equal parts, and add them into the reactor in batches. After the addition is completed, keep warm for 4 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake twice with anhydrous ethanol, disperse it in ether, stir and disperse for 40 minutes to obtain modified glass fiber.
[0056] S3. Preparation of modified basalt fiber
[0057] Put basalt fibers with a length of 10-25 mm and a diameter of 10-25 μm into a muffle furnace, raise the temperature of the muffle furnace to 480°C, keep the temperature for 3 hours, and naturally cool to room temperature to obtain heat-treated fibers;
[0058] 6 mol / L sulfuric acid, 3 mol / L nitric acid and octadecyltrimethylammonium bromide were mixed uniformly in a dosage ratio of 30 mL:50 mL:4 g to obtain a pretreatment solution for standby use;
[0059] The heat-treated fiber and the pretreatment solution were added to the reactor at a ratio of 1 g: 6 mL and stirred. The temperature of the reactor was raised to 65 ° C. The reaction was kept warm for 4 hours. The temperature of the reactor was lowered to room temperature and allowed to stand for 20 minutes. The upper suspension was skimmed off, and the lower solid was washed with purified water for 5 times and dried. The filter cake was transferred to a drying oven at a temperature of 70 ° C and dried to constant weight to obtain the pretreated fiber.
[0060] Weigh: 15 g of pretreated fiber, 50 mL of anhydrous ethanol, 15 mL of purified water and 10 mL of 6 mol / L hydrochloric acid, add into the reactor and stir, raise the temperature of the reactor to 60°C, add 10 g of triethoxy[4-(2-oxirane-1)butyl]silane into the reactor, keep warm for 2 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake into a drying oven at 60°C, and vacuum dry to constant weight to obtain modified basalt fiber.
[0061] S4. Prepare materials
[0062] The modified basalt fiber and the modified glass fiber are uniformly mixed in a weight ratio of 5:3 to obtain a composite fiber;
[0063] Coarse aggregate with a particle size of 10-20 mm, fine aggregate with a particle size of 2-8 mm, and limestone powder with a particle size of less than 2 mm are mixed in a weight ratio of 5:2:1 to obtain aggregate;
[0064] 120# solvent oil and kerosene were mixed evenly in a weight ratio of 1:3 to obtain a compatibilizer;
[0065] Dibutyl phthalate and a solubilizer are mixed uniformly in a weight ratio of 5:3 to obtain an external admixture;
[0066] The styrene-butadiene rubber and the natural rubber are uniformly mixed in a weight ratio of 1:1 to obtain rubber powder.
[0067] S5. Preparation of asphalt mixture
[0068] Weigh: 500 g of composite fiber and 5000 g of aggregate, add them into a mixer, and stir for 2 minutes to obtain a premix;
[0069] Weigh: 2500g of SMA asphalt, 250g of admixture and 500g of rubber powder and add them into a mixer. Raise the mixer temperature to 150°C and pre-mix for 30 minutes to obtain primary mixed asphalt.
[0070] The temperature of the premix is raised to 150°C. The primary mixed asphalt is slowly added to the premix under stirring. The mixture is stirred at the temperature for 45 minutes and then transferred to a heat preservation box at 150°C to obtain an asphalt mixture.
[0071] Example 2
[0072] This embodiment provides a method for preparing a composite fiber modified SMA asphalt mixture, comprising the following steps:
[0073] S1. Preparation of modifier
[0074] 70vt% ethanol, sodium hydroxide, sodium dodecyl sulfate and secondary alcohol polyoxyethylene ether were mixed uniformly in a dosage ratio of 100mL:7g:2g:1g to obtain a dispersion for later use;
[0075] Weigh: 12 g of nano iron oxide and 40 mL of dispersion liquid are added to a reactor and stirred. The temperature of the reactor is raised to 70°C. 8 g of 3-aminopropyltriethoxysilane is added to the reactor. The reaction is kept warm for 7 hours. The temperature of the reactor is lowered to room temperature. The filter cake is filtered and washed with purified water for 5 times and then with anhydrous ethanol for 2 times. The filter cake is transferred to a drying oven at 60°C and vacuum dried to constant weight to obtain a capping agent.
[0076] Weigh: 53.5 g of sodium lignin sulfonate, 27.0 g of 1,4-butanediol, and 187.3 mL of chloroform, add to a nitrogen-protected reactor and stir until the system is dissolved, add 13.4 g of N-methylmorpholine to the reactor, raise the temperature of the reactor to reflux the system, dropwise add 397.1 g of 4,4'-oxydiphthalic anhydride solution to the reactor, after the dropwise addition is complete, heat and react for 6.5 h, add 107 g of a capping agent to the reactor, heat and react for 5 h, heat and reduce the pressure to evaporate the solvent in the reactor to obtain modified sodium lignin sulfonate;
[0077] Weigh: 100 g of modified sodium lignin sulfonate and 375 mL of chloroform are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 53°C. 50 g of isocyanatepropyltriethoxysilane is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 4 hours. The reactor is kept warm at 53°C, and the solvent is evaporated under reduced pressure to obtain a modifier.
[0078] S2. Preparation of modified glass fiber
[0079] Weigh: 20 g of chopped glass fiber with a length of 20-25 mm and 200 mL of 10 wt% sodium hydroxide solution, add them into a reactor and stir, raise the temperature of the reactor to 75° C., keep warm for 2.5 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, drain, transfer the filter cake to a drying oven at a temperature of 75° C., and dry to constant weight to obtain pre-treated glass fiber;
[0080] Weigh: 15 g of pretreated glass fiber, 90 mL of anhydrous ethanol, 30 mL of purified water and 5 g of sodium hydroxide, add into the reactor and stir, raise the temperature of the reactor to 70°C, divide 20 g of the modifier into 5 equal parts, add into the reactor in batches, after the addition is complete, keep warm for 4.5 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake twice with anhydrous ethanol, disperse it in ether, stir and disperse for 40 minutes, and obtain modified glass fiber.
[0081] S3. Preparation of modified basalt fiber
[0082] Put basalt fibers with a length of 10-25 mm and a diameter of 10-25 μm into a muffle furnace, raise the temperature of the muffle furnace to 500°C, keep the temperature for 3.5 hours, and naturally cool to room temperature to obtain heat-treated fibers;
[0083] 6 mol / L sulfuric acid, 3 mol / L nitric acid and octadecyltrimethylammonium bromide were mixed uniformly in a dosage ratio of 30 mL:50 mL:4 g to obtain a pretreatment solution for standby use;
[0084] The heat-treated fiber and the pretreatment solution were added to the reactor at a ratio of 1 g: 6 mL and stirred. The temperature of the reactor was raised to 70°C and kept for 5 hours. The temperature of the reactor was lowered to room temperature and allowed to stand for 25 minutes. The upper suspension was skimmed off, and the lower solid was washed with purified water for 5 times and dried. The filter cake was transferred to a drying oven at 75°C and dried to constant weight to obtain the pretreated fiber.
[0085] Weigh: 15 g of pretreated fiber, 50 mL of anhydrous ethanol, 15 mL of purified water and 10 mL of 7 mol / L hydrochloric acid, add into the reactor and stir, raise the temperature of the reactor to 65°C, add 10 g of triethoxy[4-(2-oxirane-1)butyl]silane into the reactor, keep warm for 2.5 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake into a drying oven at a temperature of 65°C, and vacuum dry to constant weight to obtain modified basalt fiber.
[0086] S4. Prepare materials
[0087] The modified basalt fiber and the modified glass fiber are uniformly mixed in a weight ratio of 5:3 to obtain a composite fiber;
[0088] Coarse aggregate with a particle size of 10-20 mm, fine aggregate with a particle size of 2-8 mm, and limestone powder with a particle size of less than 2 mm are mixed in a weight ratio of 5:2:1 to obtain aggregate;
[0089] 120# solvent oil and kerosene were mixed evenly in a weight ratio of 1:3 to obtain a compatibilizer;
[0090] Dibutyl phthalate and a solubilizer are mixed uniformly in a weight ratio of 5:3 to obtain an external admixture;
[0091] The styrene-butadiene rubber and the natural rubber are uniformly mixed in a weight ratio of 1:1 to obtain rubber powder.
[0092] S5. Preparation of asphalt mixture
[0093] Weigh: 550 g of composite fiber and 5500 g of aggregate, add them into a mixer, and stir for 2.5 min to obtain a premix;
[0094] Weigh: 3000g of SMA asphalt, 300g of admixture and 650g of rubber powder and add them into a mixer. Raise the mixer temperature to 165°C and pre-mix for 40 minutes to obtain primary mixed asphalt.
[0095] The temperature of the premix was raised to 165°C. The primary mixed asphalt was slowly added to the premix under stirring. The mixture was stirred at the temperature for 52 minutes and then transferred to a heat preservation box at 165°C to obtain an asphalt mixture.
[0096] Example 3
[0097] This embodiment provides a method for preparing a composite fiber modified SMA asphalt mixture, comprising the following steps:
[0098] S1. Preparation of modifier
[0099] 70vt% ethanol, sodium hydroxide, sodium dodecyl sulfate and secondary alcohol polyoxyethylene ether were mixed uniformly in a dosage ratio of 100mL:7g:2g:1g to obtain a dispersion for later use;
[0100] Weigh: 12 g of nano iron oxide and 40 mL of dispersion liquid are added to a reactor and stirred. The temperature of the reactor is raised to 75°C. 8 g of 3-aminopropyltriethoxysilane is added to the reactor. The reaction is kept warm for 8 hours. The temperature of the reactor is lowered to room temperature. The filter cake is filtered and washed with purified water 5 times and then with anhydrous ethanol 2 times. The filter cake is transferred to a drying oven at a temperature of 65°C and vacuum dried to constant weight to obtain a capping agent.
[0101] Weigh: 53.5 g of sodium lignin sulfonate, 27.0 g of 1,4-butanediol, and 187.3 mL of chloroform, add them to a nitrogen-protected reactor and stir until the system is dissolved, add 13.4 g of N-methylmorpholine to the reactor, raise the temperature of the reactor to reflux the system, dropwise add 397.1 g of 4,4'-oxydiphthalic anhydride solution to the reactor, and keep the temperature for 7 h. Add 107 g of a capping agent to the reactor, keep the temperature for 6 h, keep the reactor warm and evaporate the solvent under reduced pressure to obtain modified sodium lignin sulfonate;
[0102] Weigh: 100 g of modified sodium lignin sulfonate and 375 mL of chloroform are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 55°C. 50 g of isocyanatepropyltriethoxysilane is added dropwise to the reactor. After the addition is complete, the reaction is kept warm for 5 hours. The reactor is kept warm at 55°C, and the solvent is evaporated under reduced pressure to obtain a modifier.
[0103] S2. Preparation of modified glass fiber
[0104] Weigh: 20 g of chopped glass fiber with a length of 20-25 mm and 200 mL of 10 wt% sodium hydroxide solution, add them into a reactor and stir, raise the temperature of the reactor to 80° C., keep warm for 3 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, drain, transfer the filter cake to a drying oven at a temperature of 80° C., and dry to constant weight to obtain pre-treated glass fiber;
[0105] Weigh: 15 g of pretreated glass fiber, 90 mL of anhydrous ethanol, 30 mL of purified water and 5 g of sodium hydroxide, add them into a reactor and stir, raise the temperature of the reactor to 75°C, divide 20 g of the modifier into 5 equal parts, and add them into the reactor in batches. After the addition is completed, keep warm for 5 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake twice with anhydrous ethanol, disperse it in ether, stir and disperse for 40 minutes to obtain modified glass fiber.
[0106] S3. Preparation of modified basalt fiber
[0107] Put basalt fibers with a length of 10-25 mm and a diameter of 10-25 μm into a muffle furnace, raise the temperature of the muffle furnace to 520° C., keep the temperature for 4 hours, and naturally cool to room temperature to obtain heat-treated fibers;
[0108] 6 mol / L sulfuric acid, 3 mol / L nitric acid and octadecyltrimethylammonium bromide were mixed uniformly in a dosage ratio of 30 mL:50 mL:4 g to obtain a pretreatment solution for standby use;
[0109] The heat-treated fiber and the pretreatment solution were added to the reactor at a ratio of 1 g: 6 mL and stirred. The temperature of the reactor was raised to 75°C and kept for 6 hours. The temperature of the reactor was lowered to room temperature and allowed to stand for 30 minutes. The upper suspension was skimmed off, and the lower solid was washed with purified water for 5 times and dried. The filter cake was transferred to a drying oven at 80°C and dried to constant weight to obtain the pretreated fiber.
[0110] Weigh: 15 g of pretreated fiber, 50 mL of anhydrous ethanol, 15 mL of purified water and 10 mL of 8 mol / L hydrochloric acid, add into the reactor and stir, raise the temperature of the reactor to 70°C, add 10 g of triethoxy[4-(2-oxirane-1)butyl]silane into the reactor, keep warm for 3 hours, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake into a drying oven at a temperature of 70°C, and vacuum dry to constant weight to obtain modified basalt fiber.
[0111] S4. Prepare materials
[0112] The modified basalt fiber and the modified glass fiber are uniformly mixed in a weight ratio of 5:3 to obtain a composite fiber;
[0113] Coarse aggregate with a particle size of 10-20 mm, fine aggregate with a particle size of 2-8 mm, and limestone powder with a particle size of less than 2 mm are mixed in a weight ratio of 5:2:1 to obtain aggregate;
[0114] 120# solvent oil and kerosene were mixed evenly in a weight ratio of 1:3 to obtain a compatibilizer;
[0115] Dibutyl phthalate and a solubilizer are mixed uniformly in a weight ratio of 5:3 to obtain an external admixture;
[0116] The styrene-butadiene rubber and the natural rubber are uniformly mixed in a weight ratio of 1:1 to obtain rubber powder.
[0117] S5. Preparation of asphalt mixture
[0118] Weigh: 600 g of composite fiber and 6000 g of aggregate, add them into a mixer, and stir for 3 minutes to obtain a premix;
[0119] Weigh: 3500g of SMA asphalt, 350g of admixture and 800g of rubber powder and add them into a mixer. Raise the mixer temperature to 180°C and pre-mix for 50 minutes to obtain primary mixed asphalt.
[0120] The temperature of the premix is raised to 180°C. Under stirring, the primary mixed asphalt is slowly added to the premix, stirred for 60 minutes at a temperature of 180°C, and then transferred to an insulation box for storage to obtain an asphalt mixture.
[0121] Comparative Example 1
[0122] The difference between this comparative example and Example 3 is that step S1 is eliminated, and the modified glass fiber in step S4 is replaced by the chopped glass fiber in step S2.
[0123] Comparative Example 2
[0124] The difference between this comparative example and Example 3 is that step S1 is eliminated, and the pre-treated glass fiber in step S2 replaces the modified glass fiber in step S4.
[0125] Comparative Example 3
[0126] The difference between this comparative example and Example 3 is that the modified basalt fiber in step S4 is replaced by the basalt fiber in step S3.
[0127] Comparative Example 4
[0128] The difference between this comparative example and Example 3 is that the modified basalt fiber in step S4 is replaced by the pretreated fiber in step S3.
[0129] Comparative Example 5
[0130] The difference between this comparative example and Example 3 is that no external admixture is added in step S5.
[0131] Performance Test:
[0132] The rutting resistance, shear strength, water damage resistance and freeze-thaw resistance of the asphalt mixtures prepared in Examples 1-3 and Comparative Examples 1-3 were tested, wherein the rutting resistance, water damage resistance, shear strength and freeze-thaw resistance were measured according to the standard JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" to measure the dynamic stability, Marshall modulus, water immersion residual stability and freeze-thaw splitting tensile strength ratio of the samples. The specific test results are shown in the following table:
[0133]
[0134] Data Analysis:
[0135] By comparing and analyzing the data in the above table, the dynamic stability of the asphalt mixture prepared by the present invention reaches 7296 times / mm, the Marshall modulus reaches 22.0 kN, the water immersion residual stability reaches 93.5%, the freeze-thaw splitting tensile strength ratio reaches 91.8%, and each detection performance is better than the control example, indicating that the present invention modifies the asphalt mixture by configuring an admixture, optimizes the size specifications of the glass fiber and the basalt fiber and performs surface modification on them, which not only effectively improves the rutting resistance, shear strength and freeze-thaw resistance of the asphalt mixture, but also improves the water damage resistance of the asphalt mixture.
[0136] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0137] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0138] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A composite fiber modified SMA asphalt mixture, characterized in that: The invention comprises the following components in parts by weight: 50-60 parts of composite fiber, 500-600 parts of aggregate, 25-35 parts of admixture, 250-350 parts of SMA asphalt and 50-80 parts of rubber powder; The composite fiber is composed of modified basalt fiber and modified glass fiber in a weight ratio of 5:3; The modified glass fiber is processed by the following steps: A1. Sodium lignin sulfonate, 1,4-butanediol and chloroform are added to a nitrogen-protected reactor and stirred until the system is dissolved. A catalyst is added to the reactor. The temperature of the reactor is raised to reflux. A 4,4'-oxydiphthalic anhydride solution is added dropwise to the reactor. After the addition is complete, the reaction is carried out at a temperature of 6-7 hours. A capping agent is added to the reactor. The reaction is carried out at a temperature of 4-6 hours. The modified sodium lignin sulfonate is obtained by post-treatment. A2, adding modified sodium lignin sulfonate and chloroform into a nitrogen-protected reactor and stirring, raising the temperature of the reactor to 50-55°C, adding isocyanatepropyltriethoxysilane dropwise into the reactor, and after the addition is complete, heat-retaining the reaction for 3-5 hours, and post-processing to obtain a modifier; A3, adding chopped glass fiber and activation solution into the reactor and stirring, raising the temperature of the reactor to 70-80°C, keeping the temperature for 2-3h, and post-treating to obtain pre-treated glass fiber; A4, adding pre-treated glass fiber, anhydrous ethanol, purified water and sodium hydroxide into a reactor and stirring, raising the temperature of the reactor to 65-75°C, adding modifiers into the reactor in batches, keeping the temperature for 4-5h, and post-treating to obtain modified glass fiber; In step A1, the amount ratio of sodium lignin sulfonate, 1,4-butanediol, and 4,4'-oxydiphthalic anhydride is 1 mol: 3 mol: 3.2 mol, the 4,4'-oxydiphthalic anhydride solution is composed of 4,4'-oxydiphthalic anhydride and chloroform in a weight ratio of 1:3, the amount ratio of sodium lignin sulfonate, chloroform, catalyst and end-capping agent is 2g: 7mL: 0.5g: 4g, and the catalyst is N-methylmorpholine; the post-processing operation in step A1 includes: after the reaction is completed, the reactor is kept warm, and the solvent is evaporated under reduced pressure to obtain modified sodium lignin sulfonate; in step A2, the amount ratio of modified sodium lignin sulfonate, chloroform and isocyanatepropyltriethoxysilane is 4g: 15mL: 2g; the post-processing operation in step A2 includes: after the reaction is completed, the reactor is kept warm at 50-55° C., and the solvent is evaporated under reduced pressure to obtain modifier; in step A3, the length of the chopped glass fiber is 20-25 mm, the activation solution is a 10wt% sodium hydroxide solution, and the amount ratio of the chopped glass fiber to the activation solution is 1 g: 10 mL; the post-processing operation in step A3 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed with purified water until it is neutral, and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80° C. and dried to constant weight to obtain pre-treated glass fiber; in step A4, the amount ratio of the pre-treated glass fiber, anhydrous ethanol, purified water, sodium hydroxide and modifier is 3 g: 18 mL: 6 mL: 1 g: 4 g, and the post-processing operation in step A4 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed with anhydrous ethanol twice, and then dispersed in ether, stirred and dispersed for 40 minutes to obtain modified glass fiber; The preparation method of the end-capping agent is as follows: adding nano iron oxide and a dispersion into a reaction kettle and stirring, raising the temperature of the reaction kettle to 65-75° C., adding 3-aminopropyltriethoxysilane into the reaction kettle, keeping the temperature for reaction for 6-8 hours, and post-processing to obtain the end-capping agent; The dosage ratio of the nano iron oxide, the dispersion and 3-aminopropyl triethoxysilane is 3g:10mL:2g, the dispersion is composed of 70vt% ethanol, sodium hydroxide, sodium dodecyl sulfate and secondary alcohol polyoxyethylene ether in a dosage ratio of 100mL:7g:2g:1g, and the post-treatment operation includes: after the reaction is completed, suction filtration, washing the filter cake with purified water for 5 times and then with anhydrous ethanol for 2 times, transferring the filter cake to a drying oven at a temperature of 55-65°C, and vacuum drying to constant weight to obtain a capping agent; Modified basalt fiber is processed by the following steps: B1. Put the basalt fiber into a muffle furnace, raise the temperature of the muffle furnace to 480-520°C, keep it warm for 3-4 hours, and naturally cool it down to room temperature to obtain heat-treated fiber; B2, adding the heat-treated fiber and the pretreatment solution into a reactor and stirring, raising the temperature of the reactor to 65-75°C, keeping the temperature for 4-6 hours, and post-treating to obtain the pretreated fiber; B3, adding the pretreated fiber, anhydrous ethanol, purified water and hydrochloric acid into a reactor and stirring, raising the temperature of the reactor to 60-70°C, adding triethoxy [4- (oxirane-2-yl) butyl] silane into the reactor, keeping the temperature for reaction for 2-3h, and obtaining the modified basalt fiber after post-treatment; The length of the basalt fiber in step B1 is 10-25 mm; the pretreatment solution in step B2 is composed of 6 mol / L sulfuric acid, 3 mol / L nitric acid and octadecyltrimethylammonium bromide in a dosage ratio of 30 mL: 50 mL: 4 g; the post-treatment operation in step B2 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, standing for 20-30 minutes, skimming the upper suspension, washing the lower solid with purified water for 5 times, draining, and transferring the filter cake to a drying oven at a temperature of 70-80 ° C, drying to constant weight, and obtaining the pre- Treating the fiber; in step B3, the amount ratio of the pretreated fiber, anhydrous ethanol, purified water, hydrochloric acid and triethoxy[4-(2-ethylene oxide)butyl]silane is 3g:10mL:3mL:2mL:2g, and the concentration of the hydrochloric acid is 6-8mol / L; the post-treatment operation in step B3 includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the filter is filtered, the filter cake is washed with purified water to neutrality, the filter cake is transferred to a drying oven at a temperature of 60-70°C, and vacuum dried to constant weight to obtain modified basalt fiber.
2. A composite fiber modified SMA asphalt mixture according to claim 1, characterized in that: The aggregate consists of coarse aggregate, fine aggregate and mineral powder in a weight ratio of 5:2:1, the particle size of the coarse aggregate is 10-20 mm, and the particle size of the fine aggregate is 2-8 mm; the mineral powder is limestone powder with a particle size less than 2 mm; the external admixture consists of a cosolvent and a solubilizing agent in a weight ratio of 5:3, the cosolvent is dibutyl phthalate, and the compatibilizer consists of 120# solvent oil and kerosene in a weight ratio of 1:3; the rubber powder consists of styrene-butadiene rubber and natural rubber in a weight ratio of 1:
1.
3. The method for preparing a composite fiber modified SMA asphalt mixture according to any one of claims 1-2, characterized in that: The following steps are involved: S1. Add composite fiber and aggregate into a mixer and stir for 2-3 minutes to obtain a premix; S2. Add SMA asphalt, admixtures and rubber powder into a mixer, raise the mixer temperature to 150-180°C, pre-mix for 30-50 minutes, and obtain primary mixed asphalt; S3. The temperature of the premix is raised to 150-180°C. Under stirring, the primary mixed asphalt is slowly added to the premix, stirred for 45-60 minutes under heat preservation, and then transferred to an insulation box at a temperature of 150-180°C for storage to obtain an asphalt mixture.