A nano-SiO2 modified styrene-acrylic emulsion, its preparation method and application
By preparing modified nano-SiO2-modified styrene-acrylic emulsion and combining it with cement and other components, the bonding strength and water resistance of the waterproof coating were improved. This solved the waterproof performance problem of polymer cement waterproof coatings in high temperature and high humidity environments, making it suitable for leakage protection of building structures.
Patent Information
- Application Number
- CN202311837896.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-28
AI Technical Summary
Existing polymer cement waterproof coatings have poor waterproof performance in high temperature and high humidity environments. The coating is prone to water absorption and expansion, which leads to a decrease in waterproof performance. In addition, they have poor compatibility with cement, and insufficient bonding strength and water resistance.
Surface-modified nano-SiO2 is polymerized with styrene monomers and acrylic monomers to prepare a modified nano-SiO2-modified styrene-acrylic emulsion, which is then compounded with cement, quartz sand and other components to form a waterproof coating.
It improves the bonding strength, tensile properties and water resistance of waterproof coatings, and solves the problems of poor stability and low water resistance of polymer cement waterproof coatings, making it suitable for leakage protection of building structures.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating processing technology, specifically relating to a nano-SiO2 modified styrene-acrylic emulsion, its preparation method, and its application. Background Technology
[0002] With the rapid development of the national economy, the construction industry has also developed rapidly. However, leakage in engineering projects remains a major problem affecting project quality. Leakage not only impacts structural safety and service life but also affects the functionality of buildings, causing significant inconvenience to people's lives and work. To address the problems caused by leakage, numerous researchers and engineers have made significant contributions. Currently, commercially available waterproofing products include polymer emulsion waterproof coatings, polymer cement waterproof mortar, and polymer cement waterproof coatings. Polymer cement waterproof coatings combine the flexibility of polymers with the rigidity of cement-based materials, making them the most widely used and promising waterproofing material. High-quality polymer cement waterproof materials are a key foundation for solving engineering leakage problems.
[0003] Despite years of development, polymer cement waterproof coatings have seen significant improvements in water resistance, tensile properties, low-temperature flexibility, and bond strength. However, long-term experimental research and practical experience in waterproofing projects show that, like traditional waterproof coatings, their waterproof performance still needs improvement. Furthermore, their waterproof durability is relatively poor, especially in high-temperature and high-humidity environments, where the coating easily absorbs water and expands, leading to peeling, cracking, and a decline in waterproof performance. Polymer cement coatings are composed of a liquid mixture of polymer emulsions and various additives, supplemented with powders such as cement, quartz sand, and heavy calcium carbonate. The polymer emulsion, as a crucial component, determines the coating's waterproof performance. Currently, commercially available polymer emulsions are mainly classified as styrene-acrylic emulsions, pure acrylic emulsions, and polyethylene-vinyl acetate (VAE) emulsions. Due to significant differences in synthesis processes, molecular weight distribution, and particle size among different types of emulsions, the performance of polymer waterproof coatings varies considerably depending on the emulsion system. Polymer cement waterproof coatings prepared with styrene-acrylic emulsion still have many problems, such as: poor compatibility between styrene-acrylic emulsion and cement; easy separation of organic and inorganic phases after the coating film is cured; poor long-term water resistance; the problem of the decrease in coating strength after soaking in water; and the problem of excessively high polymer-cement ratio and cost-effectiveness improvement. Summary of the Invention
[0004] To address the aforementioned issues, this invention, for the first time, utilizes surface-modified nano-SiO2 for the synthesis of styrene-acrylic emulsions and for the preparation of composite waterproof coatings.
[0005] A first aspect of the present invention provides a nano-SiO2 modified styrene-acrylic emulsion, comprising a polymer product of modified nano-SiO2, styrene monomer and acrylic monomer, wherein the modified nano-SiO2 is modified nano-SiO2 containing vinyl functional groups.
[0006] According to some embodiments of the modified styrene-acrylic emulsion of the present invention, the molar ratio of the styrene monomer to the acrylic monomer is 1:(2-5), such as 1:2, 1:3, 1:4, 1:5; the molar ratio of the styrene monomer to the modified nano-SiO2 is 1:(0.05-0.3), such as 1:0.05, 1:0.1, 1:0.2, 1:0.3.
[0007] According to some embodiments of the modified styrene-acrylic emulsion of the present invention, the modified nano-SiO2 is nano-SiO2 modified with a vinylsilane coupling agent.
[0008] According to some embodiments of the modified styrene-acrylic emulsion of the present invention, the vinyl silane coupling agent is selected from divinylbenzenesilane, vinyltriisopropoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltriacetoxysilane.
[0009] In some embodiments of the modified styrene-acrylic emulsion according to the present invention, the vinyl silane coupling agent is vinyltriisopropoxysilane.
[0010] According to some embodiments of the modified styrene-acrylic emulsion of the present invention, the acrylic monomer is methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, or glycidyl methacrylate, preferably at least one of n-butyl acrylate, 2-ethylenehexyl acrylate, and glycidyl methacrylate.
[0011] A second aspect of the present invention provides a method for preparing a modified styrene-acrylic emulsion, comprising the following steps:
[0012] Modified nano-SiO2 aqueous solution, styrene monomer, and acrylic monomer are polymerized in an aqueous solution containing an initiator and an emulsifier to obtain a modified styrene-acrylic emulsion, wherein the modified nano-SiO2 aqueous solution contains nano-SiO2 modified with a vinyl silane coupling agent.
[0013] According to some embodiments of the preparation method of the present invention, the initiator is at least one of potassium persulfate, sodium persulfate, and ammonium persulfate.
[0014] According to some embodiments of the preparation method of the present invention, the emulsifier is one of sodium lauryl ether sulfate, potassium lauryl ether sulfate, disodium salt of alkyl alcohol ether monoester, disodium salt of fatty alcohol ether sulfosuccinate, ammonium allyl alcohol oxyethylene ether sulfate, sodium allyl alcohol oxyethylene ether sulfate, and fatty alcohol polyoxyethylene ether.
[0015] According to some embodiments of the preparation method of the present invention, the acrylic monomer is at least one selected from methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and glycidyl methacrylate.
[0016] According to some embodiments of the preparation method of the present invention, the molar ratio of the styrene monomer to the acrylic monomer is 1:(2-5); the molar ratio of the styrene monomer to the modified nano-SiO2 is 1:(0.05-0.3).
[0017] According to some embodiments of the preparation method of the present invention, the modified nano-SiO2 is obtained by a preparation method comprising the following steps: reacting nano-silica and a vinylsilane coupling agent in a solvent.
[0018] According to some embodiments of the preparation method of the present invention, the modified nano-SiO2 is obtained by a preparation method including the following steps: mixing nano-silica, vinyl silane coupling agent and toluene to obtain modified nano-SiO2. Specifically, the preparation method involves: dissolving nano-silica and vinyl silane coupling agent in a toluene solution; ultrasonically dispersing the resulting mixture for 20 min to ensure uniform dispersion of the nano-silica in the solution; stirring the mixture at a constant temperature of 75°C for 15 min; then stirring with a magnetic stirrer at room temperature for 45 min to introduce vinyl functional groups into the nano-SiO2; vacuum filtering and washing the reacted solution to remove toluene and unreacted silane coupling agent; obtaining filter residue by filtration; washing the residue multiple times with anhydrous ethanol and deionized water; and then vacuum drying to obtain surface-modified nano-SiO2.
[0019] According to some embodiments of the preparation method of the present invention, the mass ratio of the nano-silica to the vinylsilane coupling agent is (6-10):(1-3), for example 6:1, 6:2, 6:3, 7:2, 8:3, 10:1, 10:2, 10:3.
[0020] According to some embodiments of the preparation method of the present invention, the reaction temperature is 15-90℃, such as 15℃, 20℃, 30℃, 40℃, 50℃, 60℃, 75℃, 80℃, and 90℃.
[0021] According to some embodiments of the preparation method described in this invention, the reaction temperature is 60-85°C.
[0022] According to some embodiments of the preparation method described in this invention, the reaction temperature is 70-80°C.
[0023] According to some embodiments of the preparation method of the present invention, the reaction time is 30-90 min, such as 30 min, 40 min, 45 min, 50 min, 60 min, 75 min, 80 min, 85 min, and 90 min.
[0024] A third aspect of the present invention provides the application of the modified styrene-acrylic emulsion described in the first aspect of the present invention or the modified styrene-acrylic emulsion obtained by the preparation method described in the second aspect of the present invention in waterproof coatings.
[0025] In a fourth aspect, the present invention provides a waterproof coating comprising a liquid component A and a powder component B;
[0026] The A component liquid includes the modified styrene-acrylic emulsion described in the first aspect of the present invention or the modified styrene-acrylic emulsion obtained by the preparation method described in the second aspect of the present invention, defoamer, dispersant, surfactant, silane coupling agent, bactericide and mildew inhibitor, and deionized water;
[0027] The B component powder includes silicate cement, quartz sand, heavy calcium carbonate powder, metakaolin, and powder water-reducing agent.
[0028] According to some embodiments of the waterproof coating of the present invention, the mass ratio of component A liquid to component B powder is 1:(1.1-1.4) (e.g., 1:1.2, 1:1.3, 1:1.4).
[0029] According to some embodiments of the waterproof coating of the present invention, the liquid component A comprises the following raw materials in parts by weight: 70-100 parts of styrene-acrylic emulsion, 1-2 parts of defoamer, 1-2 parts of dispersant, 1-1.5 parts of surfactant, 1-3 parts of silane coupling agent, 1-3 parts of bactericide and mildew inhibitor, and 8-12 parts of deionized water.
[0030] According to some embodiments of the waterproof coating of the present invention, the B component powder comprises the following raw materials in parts by weight: 40-60 parts of silicate cement, 20-40 parts of quartz sand, 15-30 parts of heavy calcium carbonate, 8-12 parts of metakaolin, and 1-2 parts of powder water-reducing agent.
[0031] According to some embodiments of the waterproof coating of the present invention, the particle size of the quartz sand is 160-400 mesh.
[0032] According to some embodiments of the waterproof coating of the present invention, the particle size of the heavy calcium carbonate is 200-400 mesh.
[0033] According to some embodiments of the waterproof coating of the present invention, the particle size of the metakaolin is 200-350 mesh.
[0034] According to some embodiments of the waterproof coating of the present invention, the silicate cement is 42.5 silicate cement.
[0035] According to some embodiments of the waterproof coating of the present invention, the defoamer is aluminum stearate, polyoxypropylene glycol ether, or mannitol.
[0036] According to some embodiments of the waterproof coating of the present invention, the dispersant is at least one selected from triethylhexylphosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, glucon, and fatty acid polyethylene glycol esters.
[0037] According to some embodiments of the waterproof coating of the present invention, the surfactant is at least one of an organosilicon twin structure surfactant (BASF, Germany) and a highly ethoxylated nonionic surfactant (Dow Chemical).
[0038] According to some embodiments of the waterproof coating of the present invention, the silane coupling agent is trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, divinylbenzene, N-hydroxymethylacrylamide, vinyltriisopropoxysilane, or polydimethylsiloxane, with polydimethylsiloxane or vinyltriisopropoxysilane being preferred.
[0039] According to some embodiments of the waterproof coating of the present invention, the bactericide and mildew inhibitor is ammonium chloride and / or hydroquinone.
[0040] According to some embodiments of the waterproof coating of the present invention, the powder water-reducing agent is a polycarboxylate superplasticizer (BASF, Germany).
[0041] According to some embodiments of the waterproof coating of the present invention, the preparation method of the waterproof coating is as follows: the liquid component A and the powder component B are mixed evenly by high-speed stirring to obtain the waterproof coating.
[0042] Compared with the prior art, the beneficial effects of the present invention are as follows: the modified styrene-acrylic emulsion of the present invention does not release small organic molecules during the film-forming and curing process, has low VOC, is green and environmentally friendly, and has broad development prospects.
[0043] The modified styrene-acrylic emulsion described in this invention, when applied to waterproof coatings, can improve the compatibility of cement and polymer emulsions, enhance the bonding strength, tensile properties, and water resistance of the waterproof coatings, and solve common technical problems in the industry such as poor stability, low water resistance, poor adhesion, low tensile strength, and poor toughness of polymer cement waterproof coatings. It can be used for balconies, roofs, kitchens, bathrooms, etc., and can effectively solve the leakage problem of building structures. Detailed Implementation
[0044] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. The specific embodiments described herein are for illustrative purposes only and are not intended to limit the invention in any way. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concepts of this disclosure. Such structures and techniques have also been described in many publications.
[0045] Example 1:
[0046] 1) By mass, 9 parts of nano-silica and 1.5 parts of divinylbenzenesilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-divinylbenzenesilane-toluene.
[0047] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0048] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0049] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0050] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0051] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0052] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0053] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0054] 9) Then cool to room temperature, adjust the pH to 8 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0055] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.2 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0056] Example 2:
[0057] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltriisopropoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltriisopropoxysilane-toluene.
[0058] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0059] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0060] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0061] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0062] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0063] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0064] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0065] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0066] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.2 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0067] Example 3
[0068] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltrimethoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltrimethoxysilane-toluene.
[0069] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0070] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce vinyl functional groups into nano-SiO2.
[0071] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0072] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0073] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0074] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0075] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0076] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0077] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.2 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0078] Example 4:
[0079] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltriethoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltriethoxysilane-toluene.
[0080] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0081] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0082] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0083] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0084] 6) Five parts of surface-modified nano-SiO2 were used in 10 parts of deionized water and ultrasonically dispersed for 20 min to prepare nano-SiO2 solution B.
[0085] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0086] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0087] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0088] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.2 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0089] Example 5:
[0090] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltriacetoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltriacetoxysilane-toluene.
[0091] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0092] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0093] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0094] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0095] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0096] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0097] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0098] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0099] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.2 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0100] Comparative Example 1
[0101] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltriisopropoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltriisopropoxysilane-toluene.
[0102] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0103] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0104] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0105] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0106] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0107] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0108] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0109] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0110] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. During use, components A and B are mixed uniformly at a high speed with a liquid-to-powder ratio of 1:1 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0111] Comparative Example 2
[0112] 1) By mass, 9 parts of nano-silica and 1.5 parts of vinyltriisopropoxysilane were dissolved in 14 parts of toluene solution to obtain a mixed solution of nano-SiO2-vinyltriisopropoxysilane-toluene.
[0113] 2) Disperse the mixed solution obtained in step 1) by ultrasonication for 20 minutes to ensure that the nano-silica in the solution is evenly dispersed.
[0114] 3) Stir the mixture at a constant temperature of 75°C for 15 min, and then stir it with a magnetic stirrer at room temperature for 45 min to introduce nano-SiO2 into the vinyl functional groups.
[0115] 4) The mixed solution after the reaction is completed is vacuum filtered and washed to remove toluene and unreacted silane coupling agent. The filter residue is obtained by filtration and washed multiple times with anhydrous ethanol and deionized water. Then, it is vacuum dried to obtain surface-modified nano-SiO2.
[0116] 5) Dissolve 0.8 parts of potassium persulfate in 10 parts of deionized water to prepare initiator solution A.
[0117] 6) Dissolve 5 parts of surface-modified nano-SiO2 in 10 parts of deionized water and ultrasonically disperse for 20 min to prepare nano-SiO2 solution B.
[0118] 7) Dissolve 3 parts sodium lauryl ether sulfate in 40 parts deionized water and heat to 90°C.
[0119] 8) Add initiator solution A, solution B, 20 parts of styrene monomer and 40 parts of acrylic monomer (acrylic acid, n-butyl acrylate and methyl methacrylate mixed in a ratio of 1:3:1) to the solution obtained in step 7). Add solution B, styrene monomer and acrylic monomer at a constant rate for 3.5 h, and add initiator solution A at a constant rate for 4.0 h, and then keep the reaction at the temperature for 1 h.
[0120] 9) Then cool to room temperature, adjust the pH to 7 with ammonia, filter out unreacted monomers, and obtain modified styrene-acrylic emulsion.
[0121] 10) A method for preparing a modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating, comprising a liquid component A and a powder component B. Liquid component A comprises 90 parts of the aforementioned modified styrene-acrylic emulsion, 1 part of polyoxypropylene propylene glycol ether, 1 part of fatty acid polyethylene glycol ester, 1.2 parts of organosilicon twin-structure surface active agent, 1 part of polydimethylsiloxane, 1 part of ammonium chloride, and 10 parts of deionized water. The powder component comprises 50 parts of 42.5 silicate cement, 30 parts of 280-mesh quartz sand, 20 parts of 280-mesh heavy calcium carbonate, 10 parts of 280-mesh metakali, and 1.5 parts of polycarboxylate superplasticizer. In use, components A and B are mixed uniformly at high speed with a liquid-to-powder ratio of 1:1.5 to obtain the modified nano-SiO2 / styrene-acrylic emulsion composite waterproof coating.
[0122] Performance testing
[0123] The particle size of the silicone-modified styrene-acrylic emulsion prepared according to this invention was measured using a Malvern Dynamic Light Scattering (DLS) instrument. The water absorption rate of the emulsion coating was determined in accordance with JC / T 1017-2006 "Polymer Emulsions for Waterproof Coatings in Buildings", GB / T16777-2008 "Test Methods for Waterproof Coatings in Buildings", and GB / T 23445-2009 "Polymer Cement Waterproof Coatings".
[0124] Table 1 shows the appearance, stability, particle size and distribution, and water absorption properties of commercially available styrene-acrylic emulsions and the modified styrene-acrylic emulsions prepared in Examples (1-5) of this invention. The results indicate that the organosilicon-modified styrene-acrylic emulsions prepared in this invention are superior to commercially available styrene-acrylic emulsions in terms of appearance, stability, emulsion particle size, and water resistance.
[0125] Table 1. Commercially available styrene-acrylic emulsions and modified styrene-acrylic emulsions prepared in Examples (1-5) of this invention.
[0126] Serial Number Appearance stability Solid content / % Particle size (d / mm) 24h water absorption rate / % Commercially available styrene-acrylic emulsion milky Six months without stratification 51% 210 18.8 Example 1 milky Six months without stratification 52.7% 270 10.2 Example 2 milky Six months without stratification 55% 265 9.1 Example 3 milky Six months without stratification 55.8% 295 11.7 Example 4 milky Six months without stratification 54.5% 280 10.8 Example 5 milky Six months without stratification 56.8% 305 12.1
[0127] The performance testing of the silicone-modified styrene-acrylic emulsion-based waterproof coating prepared in this invention was conducted in accordance with standards GB / T 16777-2008 "Test Methods for Waterproof Coatings for Buildings" and GB / T 23445-2009 "Polymer Cement Waterproof Coatings". Table 2 shows the performance test results of the JS-Ⅱ (liquid-to-powder ratio of 1:1.2) polymer cement waterproof coating prepared in some embodiments of this invention. The results indicate that the silicone-modified styrene-acrylic emulsion-based polymer cement waterproof coating possesses excellent tensile properties, adhesion properties, impermeability, and water resistance, and has broad application prospects.
[0128] Table 2 Performance test results of polymer cement waterproof coatings prepared under different example conditions
[0129]
[0130] Note: The emulsion used in the preparation method of the control sample is a commercially available styrene-acrylic emulsion.
[0131] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A nano-SiO2 modified styrene-acrylic emulsion, comprising a polymer product of modified nano-SiO2, styrene monomer and acrylic monomer, wherein the modified nano-SiO2 is nano-SiO2 modified with a vinyl silane coupling agent, and the vinyl silane coupling agent is selected from vinyltriisopropoxysilane. The molar ratio of the styrene monomer to the acrylic monomer is 1:(2-5); the molar ratio of the styrene monomer to the modified nano-SiO2 is 1:(0.05-0.3).
2. The modified styrene-acrylic emulsion according to claim 1, characterized in that, The acrylic monomers are methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, or glycidyl methacrylate.
3. The modified styrene-acrylic emulsion according to claim 1, characterized in that, The acrylic monomer is selected from at least one of n-butyl acrylate, 2-ethylenehexyl acrylate, and glycidyl methacrylate.
4. A method for preparing a modified styrene-acrylic emulsion according to any one of claims 1-3, comprising the following steps: Modified nano-SiO2 aqueous solution, styrene monomer, and acrylic monomer are polymerized in an aqueous solution containing an initiator and an emulsifier to obtain a modified styrene-acrylic emulsion. The modified nano-SiO2 aqueous solution contains nano-SiO2 modified with a vinyl silane coupling agent selected from vinyltriisopropoxysilane.
5. The preparation method according to claim 4, characterized in that, The initiator is at least one of potassium persulfate, sodium persulfate, and ammonium persulfate.
6. The preparation method according to claim 4, characterized in that, The emulsifier is one of sodium lauryl ether sulfate, potassium lauryl ether sulfate, disodium salt of fatty alcohol ether sulfosuccinate, ammonium allyl alcohol oxyethylene ether sulfate, sodium allyl alcohol oxyethylene ether sulfate, and fatty alcohol polyoxyethylene ether.
7. The preparation method according to claim 4, characterized in that, The acrylic monomer is at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and glycidyl methacrylate.
8. The preparation method according to claim 4, characterized in that, The modified nano-SiO2 is obtained by a preparation method including the following steps: reacting nano-silica and a vinyl silane coupling agent in a solvent.
9. The preparation method according to claim 8, characterized in that, The mass ratio of the nano-silica to the vinyl silane coupling agent is (6-10):(1-3).
10. The preparation method according to claim 8, characterized in that, The reaction temperature of the nano-silica and vinylsilane coupling agent in the solvent is 15-90℃.
11. The preparation method according to claim 10, characterized in that, The reaction temperature of the nano-silica and vinylsilane coupling agent in the solvent is 60-85℃.
12. The preparation method according to claim 10, characterized in that, The reaction temperature of the nano-silica and vinylsilane coupling agent in the solvent is 70-80℃.
13. The preparation method according to claim 10, characterized in that, The reaction time of the nano-silica and vinylsilane coupling agent in the solvent is 30-90 min.
14. The use of the modified styrene-acrylic emulsion according to any one of claims 1-3 or the modified styrene-acrylic emulsion obtained by the preparation method according to any one of claims 4-13 in waterproof coatings.
15. A waterproof coating comprising a liquid component A and a powder component B; The A component liquid comprises the modified styrene-acrylic emulsion according to any one of claims 1-3 or the modified styrene-acrylic emulsion obtained by the preparation method according to any one of claims 4-13, an antifoaming agent, a dispersant, a surfactant, a silane coupling agent, a bactericide and fungicide, and water; The B component powder includes silicate cement, quartz sand, heavy calcium carbonate, metakaolin, and powder water-reducing agent.
16. The waterproof coating according to claim 15, characterized in that, The mass ratio of component A liquid to component B powder is 1:(1.1-1.4).
17. The waterproof coating according to claim 15, characterized in that, The A component liquid comprises the following raw materials in parts by weight: 70-100 parts of styrene-acrylic emulsion, 1-2 parts of defoamer, 1-2 parts of dispersant, 1-1.5 parts of surfactant, 1-3 parts of silane coupling agent, 1-3 parts of bactericide and mildew inhibitor, and 8-12 parts of deionized water.
18. The waterproof coating according to claim 15, characterized in that, The B component powder comprises the following raw materials in parts by weight: 40-60 parts silicate cement, 20-40 parts quartz sand, 15-30 parts heavy calcium carbonate, 8-12 parts metakaolin, and 1-2 parts powder water-reducing agent.
19. The waterproof coating according to claim 15, characterized in that, The quartz sand has a particle size of 160-400 mesh.
20. The waterproof coating according to claim 15, characterized in that, The particle size of the calcium carbonate is 200-400 mesh.
21. The waterproof coating according to claim 15, characterized in that, The particle size of the metakaolin is 200-350 mesh.
22. The waterproof coating according to claim 15, characterized in that, The defoamer is aluminum stearate, polyoxypropylene glycol ether, or mannitol; And / or, the dispersant is at least one of triethylhexylphosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, glucon, and fatty acid polyethylene glycol esters; And / or, the surfactant is an organosilicon twin structure surfactant; And / or, the silane coupling agent is vinyltriisopropoxysilane or polydimethylsiloxane; And / or, the bactericide and antifungal agent is ammonium chloride and / or hydroquinone.
23. The waterproof coating according to claim 15, characterized in that, The powder water-reducing agent is a polycarboxylate high-efficiency water-reducing agent.
Citation Information
Patent Citations
Waterproof paint and preparation method thereof
CN104446192A