A method for preparing high-silicon steel strip containing cerium (Fe-6.5 wt.%) Si using a single-roller spinning method.

By adding cerium to high-silicon steel using a single-roller spinning method, the brittleness problem of Fe-6.5wt.%Si high-silicon steel strip was solved, enabling efficient and low-cost preparation of high-performance strips. This simplified the process and improved the yield and performance.

CN118028686BActive Publication Date: 2026-11-10NORTHEASTERN UNIV CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410072245.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-18
Publication Date
2026-11-10
Estimated Expiration
2044-01-18

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively prepare high-silicon steel strips, especially Fe-6.5wt.%Si high-silicon steel strips. Problems include the generation of brittle ordered phases, low material toughness, complex production process, and high cost. Furthermore, research on adding Ce in rapid solidification processes has not been reported.

Method used

Cerium was added to a high-silicon steel system using a single-roller spinning method, and Fe-6.5wt.%Si high-silicon steel strip was prepared through a rapid solidification process. The specific steps included melting, single-roller spinning, and rapid cooling. The nozzle shape, size, and spraying parameters were controlled to ensure uniform distribution of Ce.

Benefits of technology

The preparation of Fe-6.5wt.%Si high-silicon steel strips with high plasticity and high magnetic properties has been achieved, simplifying the process, improving the yield, reducing production costs, and avoiding segregation and complex steps in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118028686B_ABST
    Figure CN118028686B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of metal material preparation technology and discloses a method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strips using a single-roller spinning method. The chemical composition, by mass percentage, is: Si: 6.3%–6.6%, Ce: 0.006%–0.08%, S≤0.01%, B≤0.002%, Mn≤0.007%, P≤0.008%, with the balance being Fe and unavoidable impurities. This invention utilizes single-roller spinning technology to add 0.006%–0.08% Ce to Fe-6.5wt.%Si high-silicon steel, resulting in a reduction of ordered phases and an increase in tensile strength and elongation. The addition of trace amounts of rare earth elements to the Fe-6.5wt.%Si high-silicon steel strips achieves deep purification, grain refinement, and micro-alloying, while reducing the formation of ordered phases in the high-silicon steel, significantly improving the plasticity and magnetic properties of the Fe-6.5wt.%Si high-silicon steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material preparation technology, specifically relating to a method for preparing cerium-containing Fe-6.5wt.%Si high silicon steel strips by a single-roller spinning method. Background Technology

[0002] Fe-6.5wt.%Si high-silicon steel possesses excellent soft magnetic properties such as high magnetic permeability, high frequency and low iron loss, and a near-zero magnetostriction coefficient, making it an important magnetic material for the power and telecommunications industries in manufacturing generators, motors, transformers, instrument transformers, relays, and other electrical instruments. However, as the Si content increases, high-silicon steel easily forms brittle ordered phases B2 and DO3, significantly reducing the material's room temperature toughness and making it difficult to process using conventional methods, thus hindering its widespread application. Although Japan has achieved mass industrial production of Fe-6.5wt.%Si high-silicon steel strips using chemical vapor deposition, a series of problems, including high equipment wear and tear, high costs, heavy pollution, and low production efficiency, cannot be ignored.

[0003] Rare earth elements have unique atomic structures and highly reactive chemical properties. Their addition to various metallic materials can significantly influence the mechanical, physical, and chemical properties of alloys through their effects on microstructure, structure, and phase transformations. The role of rare earth elements in steel can generally be summarized as purification, modification, and microalloying. Numerous studies on various steel grades have demonstrated that trace amounts of rare earth elements can effectively improve the impact toughness and plasticity of carbon steel, low-alloy steel, and alloy steel. The application of adding rare earth element Ce to silicon steel to improve its properties has also been reported in the traditional production process of high-silicon steel.

[0004] Chinese invention patent publication number CN101358272A discloses a method for preparing high-grade non-oriented electrical steel with added rare earth cerium. This invention uses high-Si, rare earth Ce-added non-oriented electrical steel billets as hot-rolled raw materials, and performs processes such as hot rolling, normalizing, pickling, cold rolling, annealing, and coating to obtain high-grade non-oriented electrical steel products with good magnetic properties. This production method provides some specific process routes for strengthening high-grade non-oriented electrical steel and has certain reference value. However, its production process is complex and costly, and it requires a normalizing process, which is detrimental to resource conservation and environmental development. Chinese invention patent publication number CN111155023B discloses a method for preparing high-toughness, high-strength, non-oriented, high-silicon steel. It involves vacuum smelting, ten-roll hot rolling, normalizing, high-temperature heat treatment, cooling and water quenching, low-temperature annealing, pickling, and coating to obtain products with good toughness and strength. However, it involves too many types of added elements, making it difficult to control the dosage, and the production process is complex and costly.

[0005] The single-roller belt spinning method, characterized by rapid solidification, can generate new metastable phases, increase the solubility of solid solutions, and eliminate compositional segregation in some alloy systems, thus significantly improving the microstructure and properties of certain materials, and has therefore experienced rapid development. Rapid solidification technology for preparing high-magnetic-performance silicon steel offers advantages not found in other processes, such as short process time, high efficiency, and energy saving and environmental friendliness. Although some studies have shown that adding Ce to high-silicon steel under traditional preparation conditions can improve its properties, research on the preparation of Ce-containing high-silicon steel under rapid solidification conditions has not yet been reported. Summary of the Invention

[0006] To address the problems existing in the prior art, this invention discloses a method for preparing cerium-containing Fe-6.5wt.%Si high silicon steel strips using a single-roller spinning method.

[0007] The technical solution of this invention is:

[0008] A method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strips using a single-roller spinning process involves adding a certain amount of cerium to a high-silicon steel system and then using a single-roller spinning process to prepare high-ductility and high-magnetic-performance high-silicon steel strips. The specific steps are as follows:

[0009] (1) Selection of raw materials: Industrial pure iron with a purity of 99.9 wt.%, metallic silicon with a silicon content of 99.9 wt.%, and metallic cerium with a cerium content of 99.9 wt.% are used as raw materials;

[0010] (2) Smelting: High silicon steel ingots are prepared by arc melting in a high vacuum arc melting furnace. The chemical composition of the ingots by mass percentage is: Si: 6.3%~6.6%, Ce: 0.006%~0.08%, S≤0.01%, B≤0.002%, Mn≤0.007%, P≤0.008%, with the balance being Fe and unavoidable impurities.

[0011] (3) Single-roller strip casting: The polished ingot is placed in a crucible with holes at the bottom for induction melting. After the alloy is completely melted into liquid metal, the molten liquid is sprayed onto a rotating copper roller through a nozzle using inert gas for strip casting. After rapid cooling, Fe-6.5wt.%Si high silicon steel strip is obtained.

[0012] Furthermore, in the above-mentioned method for preparing high silicon steel strip containing cerium Fe-6.5wt.%Si by single-roller spinning, the raw material composition in step (1) is as follows by weight ratio: Si: 6.3-6.6%, Ce: 0.006-0.08%, with the remainder being Fe and unavoidable impurities.

[0013] Furthermore, in the above-mentioned method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning, the high-silicon steel ingot in step (2) is remelted at least four times to ensure uniform composition.

[0014] Furthermore, in the above-mentioned method for preparing cerium-containing Fe-6.5wt.%Si high silicon steel strip by single-roller spinning, the inert gas in step (3) includes, but is not limited to, high-purity argon.

[0015] Furthermore, in the above-mentioned method for preparing cerium-containing Fe-6.5wt.%Si high silicon steel strip by single-roller casting, the temperature of the molten liquid in step (3) when the molten liquid is sprayed onto the rotating copper roller through a nozzle is 1450~1700℃.

[0016] Furthermore, in the above-mentioned method for preparing cerium-containing Fe-6.5wt.%Si high silicon steel strip by single-roller spinning, the type of nozzle in step (3) of single-roller spinning includes, but is not limited to, a circular nozzle. The diameter of the circular or conical nozzle is Z0.3-5mm, the width of the rectangular or arc-shaped nozzle is controlled at 5-15mm, the nozzle gap size is controlled at 0.1-3mm, the distance between the nozzle and the copper roller is 0.1-10mm, the pressure of the nozzle during spraying is 0.03-0.2MPa, and the rotation speed of the copper roller is 20-60m / s.

[0017] Furthermore, the above-mentioned method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strips by single-roller spinning yields Fe-6.5wt.%Si high-silicon steel strips with a thickness range of 35–45 μm.

[0018] Advantages and beneficial effects of the present invention:

[0019] This invention employs a rapid solidification single-roller spinning process to directly and rapidly cool molten metal and spin it into a Fe-6.5wt.%Si high-silicon steel strip. The nozzle shape and size, the distance between the nozzle and the copper roller, and the injection pressure were determined through extensive experimentation. The cerium-containing silicon steel strip system has a composition of Fe-(6.3-6.4)wt.%Si-(0.006-0.08)wt.%Ce, and the Si and Ce content was verified and matched through extensive experimentation. Its advantages are as follows:

[0020] (1) Adding a small amount of Ce to Fe-6.5wt.%Si high silicon steel strip can effectively suppress the generation of ordered phase and improve its plasticity;

[0021] (2) Compared with traditional preparation methods, the addition of a certain amount of Ce element to Fe-6.5wt.%Si high silicon steel strip by single-roller spinning method will not cause segregation, the Ce element is evenly distributed, and the yield is high.

[0022] (3) It eliminates the complicated hot rolling and cold rolling steps of traditional process for preparing Fe-6.5wt.%Si high silicon steel strip, making the process simple and the process short;

[0023] (4) Streamlined steps, high preparation efficiency, high product precision, no pollution or inclusions, and excellent performance. Attached Figure Description

[0024] Figure 1 This is the rare earth-free and 0.029 wt.% Ce Fe-6.5 wt.% Si high-silicon steel strip provided in Example 1 of the present invention. <011> Zone axis diffraction pattern and (200) dark field image;

[0025] In the figure: (a) No rare earth elements <011> Zone axis diffraction pattern; (b) 0.029 wt.% Ce <011> Zone axis diffraction pattern; (c) Dark field image without rare earth elements (200); (d) Dark field image with 0.029 wt.% Ce (200);

[0026] Figure 2 This is a schematic diagram of the tensile stress-strain curves of rare earth-free and high-silicon steel strips containing 0.029 wt.% CeFe-6.5 wt.% Si provided in Embodiment 1 of the present invention.

[0027] Figure: (a) Tensile stress of rare earth-free Fe-6.5wt.%Si high silicon steel strip (a) Strain curves; (b) Tensile stress-strain curves of 0.029 wt.% CeFe-6.5 wt.% Si high silicon steel strip;

[0028] Figure 3 This is a schematic diagram of the tensile fracture morphology of a rare earth-free and 0.029wt.%CeFe-6.5wt.%Si high-silicon steel strip provided in Embodiment 1 of the present invention;

[0029] Figure: (a) Tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strip without rare earth additives; (b) Tensile fracture morphology of 0.029wt.%Ce-6.5wt.%Si high silicon steel strip.

[0030] Figure 4 This is a schematic diagram of the tensile stress-strain curves of rare earth-free and high-silicon steel strips containing 0.019 wt.% CeFe-6.5 wt.% Si provided in Embodiment 2 of the present invention.

[0031] In the figure: (a) Tensile stress-strain curve of Fe-6.5wt.%Si high silicon steel strip without rare earth; (b) Tensile stress-strain curve of 0.019wt.%CeFe-6.5wt.%Si high silicon steel strip;

[0032] Figure 5This is a schematic diagram of the tensile fracture morphology of a rare earth-free and 0.019wt.%CeFe-6.5wt.%Si high-silicon steel strip provided in Embodiment 2 of the present invention;

[0033] Figure: (a) Tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strip without rare earth additives; (b) Tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strip with 0.019wt.%Ce.

[0034] Figure 6 This is a schematic diagram of the tensile stress-strain curves of rare earth-free and high-silicon steel strips containing 0.073 wt.% CeFe-6.5 wt.% Si provided in Embodiment 3 of the present invention.

[0035] In the figure: (a) Tensile stress-strain curve of Fe-6.5wt.%Si high silicon steel strip without rare earth; (b) Tensile stress-strain curve of 0.073wt.%CeFe-6.5wt.%Si high silicon steel strip;

[0036] Figure 7 This is a schematic diagram of the tensile fracture morphology of a rare earth-free and 0.073wt.%CeFe-6.5wt.%Si high-silicon steel strip provided in Embodiment 3 of the present invention;

[0037] Figure: (a) Tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strip without rare earth additives; (b) Tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strip with 0.073wt.%Ce. Detailed Implementation

[0038] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention.

[0039] Example 1

[0040] This invention provides a method for preparing high-silicon steel strip containing 0.029 wt.% CeFe-6.5 wt.% Si using a single-roller spinning method. The specific process steps are as follows:

[0041] (1) Smelting: The first step is carried out in a high vacuum electric arc melting and suction casting system. Pure iron and alloy elemental silicon and cerium are mixed and melted, and then cooled after electromagnetic stirring to obtain high silicon steel ingots. The chemical composition of the ingots by mass percentage is: Si: 6.34%, Ce: 0.029%, S: 0.08%, B: 0.002%, Mn: 0.005%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0042] (2) Single-roller strip casting: The polished ingot is placed in a crucible with holes at the bottom for induction melting. After the alloy is completely melted into liquid metal, the molten liquid is sprayed through a nozzle onto a rotating copper roller for strip casting. After rapid cooling, a Fe-6.5wt.%Si high silicon steel strip with a thickness of 40-43μm is obtained.

[0043] In the preferred embodiment 1 of the present invention, the high-silicon steel ingot is remelted four times to ensure uniform composition.

[0044] In a preferred embodiment 1 of the present invention, the inert gas used is argon, and the injection pressure is 0.04 MPa.

[0045] In a preferred embodiment 1 of the present invention, when the molten liquid is sprayed onto the rotating copper roller through a nozzle, the temperature of the molten liquid is 1550-1650°C.

[0046] In the preferred embodiment 1 of the present invention, the nozzle size is a circular nozzle with a nozzle orifice diameter of φ1mm, the distance between the nozzle and the copper roller is 8-10mm, and the rotational speed of the copper roller is 30m / s.

[0047] The application effects of this invention will be described in detail below based on the test results.

[0048] like Figure 1 As shown, a comparison is made between rare earth-free and high-silicon steel strips containing 0.029 wt.% CeFe-6.5 wt.% Si. <011> The zone axis diffraction pattern and (200) dark field image clearly show that the addition of rare earth Ce reduces the ordered phase and decreases the degree of order.

[0049] like Figure 2 As shown, comparing the tensile stress-strain curves of high-silicon steel strips with and without rare earth elements (containing 0.029 wt.% CeFe-6.5 wt.% Si), it is evident that the tensile strength and elongation are significantly improved after adding rare earth element Ce.

[0050] like Figure 3 As shown, comparing the tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strips without rare earth and those containing 0.029wt.%Ce, it is obvious that the number of dimples increases and the dimples are larger and deeper after adding rare earth Ce. It can be seen that the addition of 0.029wt.%Ce improves the room temperature tensile toughness and plasticity of Fe-6.5wt.%Si high silicon steel strips.

[0051] The main mechanical and magnetic properties of the high-silicon steel strip containing 0.029wt.%CeFe-6.5wt.%Si in this embodiment are shown in Table 1. It can be seen that the tensile strength, yield strength and elongation of the strip are improved, its saturation magnetization is improved and its coercivity is reduced.

[0052] Example 2

[0053] This invention provides a method for preparing high-silicon steel strip containing 0.019 wt.% CeFe-6.5 wt.% Si using a single-roller spinning method. The specific process steps are as follows:

[0054] (1) Smelting: The first step is carried out in a high vacuum electric arc melting furnace. Pure iron and alloy elemental silicon and cerium are mixed and melted, and then cooled after electromagnetic stirring to obtain high silicon steel ingots. The chemical composition of the ingots by mass percentage is: Si: 6.34%, Ce: 0.019%, S: 0.009%, B: 0.001%, Mn: 0.005%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0055] (2) Single-roller strip casting: The polished ingot is placed in a crucible with holes at the bottom for induction melting. After the alloy is completely melted into liquid metal, the molten liquid is sprayed through a nozzle onto a rotating copper roller for strip casting. After rapid cooling, a Fe-6.5wt.%Si high silicon steel strip with a thickness of 40-45μm is obtained.

[0056] In the preferred embodiment 2 of the present invention, the high-silicon steel ingot is remelted four times to ensure uniform composition.

[0057] In the preferred embodiment 2 of the present invention, the inert gas used is argon, and the injection pressure is 0.04 MPa.

[0058] In a preferred embodiment 2 of the present invention, when the molten liquid is sprayed onto the rotating copper roller through a nozzle, the temperature of the molten liquid is 1550-1650°C.

[0059] In the preferred embodiment 2 of the present invention, the nozzle size is a circular nozzle with a nozzle orifice diameter of φ1mm, the distance between the nozzle and the copper roller is 10mm, and the rotational speed of the copper roller is 30m / s.

[0060] The application effects of this invention will be described in detail below based on the test results.

[0061] like Figure 4 As shown, the tensile stress of high-silicon steel strips with no rare earth elements and containing 0.019 wt.% CeFe-6.5 wt.% Si is compared. The strain curves clearly show that the addition of rare earth element Ce improves both tensile strength and elongation.

[0062] like Figure 5 As shown, comparing the tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strips without rare earth and those containing 0.019wt.%Ce, it is obvious that the number of dimples increases after adding rare earth Ce, indicating that adding 0.019wt.%Ce improves the room temperature tensile toughness and plasticity of Fe-6.5wt.%Si high silicon steel strips.

[0063] The main mechanical and magnetic properties of the high-silicon steel strip containing 0.019wt.%CeFe-6.5wt.%Si in this embodiment are shown in Table 1. It can be seen that the tensile strength, yield strength and elongation of the strip are improved, its saturation magnetization is improved and its coercivity is reduced.

[0064] Example 3

[0065] This invention provides a method for preparing high-silicon steel strip containing 0.073 wt.% CeFe-6.5 wt.% Si using a single-roller spinning method, comprising smelting and spinning processes, the specific process steps of which are as follows:

[0066] (1) Smelting: The first step is carried out in a high vacuum electric arc melting furnace. Pure iron and alloy elemental silicon and cerium are mixed and melted, and then cooled after electromagnetic stirring to obtain high silicon steel ingots. The chemical composition of the ingots by mass percentage is: Si: 6.35%, Ce: 0.073%, S: 0.008%, B: 0.001%, Mn: 0.007%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0067] (2) Single-roller strip casting: The polished ingot is placed in a crucible with holes at the bottom for induction melting. After the alloy is completely melted into liquid metal, the molten liquid is sprayed onto a rotating copper roller through a nozzle using an inert gas for strip casting. After rapid cooling, a Fe-6.5wt.%Si high silicon steel strip with a thickness of 40-44μm is obtained.

[0068] In the preferred embodiment 3 of the present invention, the high-silicon steel ingot is remelted four times to ensure uniform composition.

[0069] In the preferred embodiment 3 of the present invention, the inert gas used is argon, and the injection pressure is 0.04 MPa.

[0070] In a preferred embodiment 3 of the present invention, when the molten liquid is sprayed onto the rotating copper roller through a nozzle, the temperature of the molten liquid is 1550-1650°C.

[0071] In the preferred embodiment 3 of the present invention, the nozzle size is a circular nozzle with a nozzle orifice diameter of φ1mm, the distance between the nozzle and the copper roller is 10mm, and the rotational speed of the copper roller is 30m / s.

[0072] The application effects of this invention will be described in detail below based on the test results.

[0073] like Figure 6 As shown, the tensile stress of high-silicon steel strips with no rare earth elements and containing 0.073 wt.% CeFe-6.5 wt.% Si is compared. The strain curves clearly show that the addition of rare earth element Ce improves both tensile strength and elongation.

[0074] like Figure 7 As shown, comparing the tensile fracture morphology of Fe-6.5wt.%Si high silicon steel strips without rare earth and those containing 0.019wt.%Ce, it is obvious that the number of dimples increases after adding rare earth Ce, indicating that adding 0.019wt.%Ce improves the room temperature tensile toughness and plasticity of Fe-6.5wt.%Si high silicon steel strips.

[0075] The main mechanical and magnetic properties of the high-silicon steel strip containing 0.073wt.%CeFe-6.5wt.%Si in this embodiment are shown in Table 1. It can be seen that the tensile strength, yield strength and elongation of the strip are improved, its saturation magnetization is improved and its coercivity is reduced.

[0076] Table 1. Main mechanical and magnetic properties of CeFe-6.5wt.%Si high-silicon steel strips in Examples 1-3

[0077]

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strips using a single-roller spinning method, characterized in that, A certain amount of cerium element is added to a high-silicon steel system, and a high-silicon steel thin strip with high plasticity and high magnetic properties is prepared by single-roller spinning process. The specific steps are as follows: (1) Selection of raw materials: Industrial pure iron with a purity of 99.9 wt.%, metallic silicon with a silicon content of 99.9 wt.%, and metallic cerium with a cerium content of 99.9 wt.% were used as raw materials; (2) Smelting: High silicon steel ingots are prepared by arc melting in a high vacuum arc melting furnace. The chemical composition of the ingots by mass percentage is: Si: 6.3%~6.6%, Ce: 0.006%~0.08%, S≤0.01%, B≤0.002%, Mn≤0.007%, P≤0.008%, with the balance being Fe and unavoidable impurities; (3) Single-roller strip casting: The polished ingot is placed in a crucible with holes at the bottom for induction melting. After the alloy is completely melted into liquid metal, the molten liquid is sprayed onto a rotating copper roller through a nozzle using inert gas for strip casting. After rapid cooling, Fe-6.5wt.%Si high silicon steel strip is obtained. The type of nozzles in the single-roller belt spinning step (3) includes, but is not limited to, circular nozzles. The diameter of the circular or conical nozzle is φ0.3 to 5 mm, the width of the rectangular or arc-shaped nozzle is controlled at 5 to 15 mm, the nozzle gap size is controlled at 0.1 to 3 mm, the distance between the nozzle and the copper roller is 0.1 to 10 mm, the pressure of the nozzle during spraying is 0.03 to 0.2 MPa, and the rotation speed of the copper roller is 20 to 60 m / s.

2. The method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning according to claim 1, characterized in that, Step (1) The raw material composition by weight ratio is: Si: 6.3-6.6%, Ce: 0.006-0.08%, and the remainder is Fe and unavoidable impurities.

3. The method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning according to claim 1, characterized in that, The high-silicon steel ingot described in step (2) is remelted at least four times to ensure uniform composition.

4. The method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning according to claim 1, characterized in that, The inert gas mentioned in step (3) includes, but is not limited to, high-purity argon.

5. The method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning according to claim 1, characterized in that, In step (3), when the molten liquid is sprayed onto the rotating copper roller through a nozzle, the temperature of the molten liquid is 1450-1700 ℃.

6. The method for preparing cerium-containing Fe-6.5wt.%Si high-silicon steel strip by single-roller spinning according to claim 1, characterized in that, The thickness range of Fe-6.5wt.%Si high silicon steel strips obtained is 35–45 μm.

Citation Information

Patent Citations

  • Method for preparing high grade non-oriented electrical steel adding rare earth cerium

    CN101358272A

  • Preparation method of high toughness, high strength, non-oriented high silicon steel

    CN111155023B

  • Strong-magnetic-induction nanocrystalline high-silicon steel wire material and preparation method thereof