A self-melting ice ultra-thin wear layer material and its preparation method and application
By applying a combination of hydrophobic ice-suppressing coating, anti-slip ice-breaking wear layer and conductive anti-icing membrane layer on the road, the problem of ice and snow affecting road safety in winter is solved, achieving efficient snow and ice melting and reducing environmental pollution.
Patent Information
- Application Number
- CN202410348813.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Black ice on roads caused by ice and snow in winter is difficult to detect, and traditional snow melting agents have problems with environmental pollution and high construction difficulty, which affects road driving safety.
The self-melting ice ultra-thin wear layer material composed of a hydrophobic ice-suppressing coating, an anti-slip ice-breaking wear layer and a conductive anti-icing membrane layer improves the efficiency of melting snow and ice through hydrophobicity, anti-slip properties and conductive heating properties, reducing the freezing point and enhance road safety.
It improves the hydrophobicity and deicing efficiency of the road, reduces the difficulty of construction, enhances the safety performance of the road, and realizes efficient snow and ice melting through the heating function of the conductive anti-icing membrane layer, reducing environmental pollution.
Smart Images

Figure CN118029222B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering, and in particular relates to a self-melting ice ultra-thin wear layer material and a preparation method and application thereof. Background Art
[0002] More than 70% of China's roads are affected by winter ice and snow. In particular, there is a thin black ice that is hard to detect on the road. Due to its thin thickness, the color of the road itself will be reflected through it, resulting in low visibility of the ice surface and extremely difficult to detect. At the same time, because its temperature is not low, there is a layer of melted water on the surface of the ice, making this ice more slippery than thick ice with a lower temperature. Black ice is generally formed after a light rain, when the temperature is below 0 degrees Celsius, when the road surface with accumulated water undergoes rapid freezing, or when supercooled (liquid below freezing point but not frozen) fog is blocked by buildings or vegetation. Among them, bridges are the most likely to form black ice. Since bridges are overhead, the air flowing up and down can easily take away heat, making the bridge deck more susceptible to heat loss. "Black ice" can cause vehicles to lose control, skid, spin, and significantly extend the braking distance. According to statistics, in the past five years, the number of traffic accidents caused by black ice in South Korea is four times that of ordinary ice and snow, and there are more than 150,000 traffic accidents caused by frozen roads in the United States every year, and more than 550 people lose their lives.
[0003] Although traditional chemical deicing agents can achieve the effect of melting snow and ice to a certain extent, the damage to roads and bridges is irreversible. Some chemical substances may flow into groundwater or soil during the snow melting process, causing irreversible impacts on the environment. In addition, the traditional deicing agent method belongs to passive deicing, which has hysteresis and low efficiency. At present, active deicing methods mainly use heat pipe heating and cable heating methods. Although these methods can effectively deicer to a certain extent, these methods have the problem of high construction difficulty. Therefore, it is urgent to study the road deicing technology. Summary of the invention
[0004] In order to solve the problem of winter ice and snow affecting road driving safety, the present invention proposes a self-melting ice ultra-thin wear layer material and its preparation method and application. When the self-melting ice ultra-thin wear layer material of the present invention is applied to roads, it can improve the efficiency of snow and ice melting and enhance the safety of winter roads.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A self-melting ice ultra-thin wear layer material, which consists of a hydrophobic ice-suppressing coating, an anti-skid ice-breaking wear layer and a conductive anti-ice coil layer;
[0007] The anti-skid and ice-breaking wear layer is located between the hydrophobic ice-suppressing coating and the conductive anti-ice coiled material layer.
[0008] Furthermore, the thickness of the hydrophobic ice-suppressing coating is 0.1 to 0.5 mm, the thickness of the anti-skid and ice-breaking wear layer is 3 to 6 mm, and the thickness of the conductive anti-ice coil layer is 0.1 to 0.5 mm. The self-melting ice ultra-thin wear layer material of the present invention is thin in overall thickness and conductive, and is suitable for new and existing roads.
[0009] Furthermore, the hydrophobic anti-icing coating comprises the following raw materials in percentage by mass: 8-15% silicone rubber solution, 8-15% potassium carbonate, 3-8% alkaline silica sol, 0.5-1% methyl silicone oil, 0.8-1.5% SBS modified asphalt, 70-80% water, 0.5-0.8% methyl silicate and 0.1-0.3% accelerator.
[0010] Furthermore, the organic silicone rubber solution is octamethylcyclotetrasiloxane; the alkaline silica sol is a silica colloidal solution; and the accelerator is accelerator D.
[0011] Furthermore, the preparation method of the hydrophobic anti-icing coating is as follows: accurately weigh each raw material according to the mass percentage, mix and stir evenly to obtain a hydrophobic coating raw material mixture, add sodium chloride, sodium acetate and corrosion inhibitor to the hydrophobic coating raw material mixture, and obtain the hydrophobic anti-icing coating after coating.
[0012] Furthermore, the amount of sodium chloride added is 4-6% of the total mass of the hydrophobic anti-icing coating raw material, the amount of sodium acetate added is 4-6% of the total mass of the hydrophobic anti-icing coating raw material, and the amount of corrosion inhibitor added is 0.5-1% of the total mass of the hydrophobic anti-icing coating raw material.
[0013] Furthermore, the corrosion inhibitor is a BTA corrosion inhibitor. Adding the corrosion inhibitor to the coating can play an anti-corrosion role and prolong the effect of the hydrophobic ice-inhibiting layer. The role of sodium chloride and sodium acetate can not only reduce the freezing point, but also enhance the adhesion of the overall coating; the silicon-containing raw material can not only play a hydrophobic role, but also improve the wear resistance of the hydrophobic ice-inhibiting layer; potassium carbonate plays a role in reducing the freezing point; accelerator D can not only accelerate the reaction speed, but also improve the adhesion of the coating; SBS modified asphalt plays a bonding role.
[0014] Furthermore, the raw materials of the conductive anti-icing coiled material layer include: carbon fiber cloth, copper sheet, conductive adhesive material and low freezing point sealing glue.
[0015] Furthermore, the carbon fiber cloth is 3K carbon fiber cloth, and the copper sheet is a red copper sheet. The carbon fiber cloth is a conductive heating material, and the copper sheet electrode transmits current.
[0016] Furthermore, the preparation method of the conductive adhesive material is as follows: polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed in a mass ratio of 75:(10-15):(10-12):(1-2):(0.5-1), and stirred evenly to obtain the conductive adhesive material; polyurethane acrylate is a matrix resin material, which can improve the adhesion of the conductive adhesive material, lauryl methacrylate is a monomer material and can improve the water resistance of the conductive adhesive material, isocyanate is a cross-linking agent material, which can not only play a cross-linking role, but also improve the durability of the conductive adhesive material and extend the life of the overall conductive anti-icing coil material layer, tert-butyl perbenzoate is a thermal initiator material, which reacts with the monomer to form a resin, further improving the adhesion of the glue, and epoxy phosphate is an adhesion promoter material.
[0017] The preparation method of the low freezing point seal glue is as follows: adding a low freezing point material and a corrosion inhibitor to a two-component polyurethane glue to obtain a low freezing point polyurethane glue, and then adding polyethylene glycol, stirring evenly, to obtain the low freezing point seal glue. Adding a low freezing point material can lower the freezing point to achieve an anti-icing effect, and polyethylene glycol as a phase change material can release heat to improve the ice melting ability of the road surface. The polyurethane glue is a flexible material that can seal the entire conductive material and is designed in the form of a coil.
[0018] Furthermore, the polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed at a rotation speed of 400 r / min for 30 minutes.
[0019] Furthermore, the low freezing point material is sodium chloride and sodium acetate; the corrosion inhibitor is BTA corrosion inhibitor; and the polyethylene glycol is PEG-2000.
[0020] Furthermore, the amount of sodium chloride added is 4-6% of the total mass of the two-component polyurethane glue; the amount of sodium acetate added is 4-6% of the total mass of the two-component polyurethane glue; the amount of corrosion inhibitor added is 0.5-1% of the total mass of the two-component polyurethane glue; the amount of polyethylene glycol added is 10-12% of the total mass of the two-component polyurethane glue.
[0021] Furthermore, the preparation method of the two-component polyurethane glue is as follows: stirring for 120 seconds at room temperature according to the mass ratio of A:B=(8-10):(3-5) to obtain the two-component polyurethane glue, wherein component A is a water-based polyurethane resin and component B is trimethylolpropane.
[0022] Furthermore, the preparation method of the conductive anti-icing coil material layer is as follows:
[0023] Drying the carbon fiber cloth;
[0024] The surfaces of two copper sheets are polished and ground to serve as electrodes;
[0025] Apply a conductive adhesive material on the inner side of the electrode, fold the electrode in half along the wide side, sandwich the dried carbon fiber cloth between the two folded electrodes, compact them, and install two copper sheet electrodes on both sides of the carbon fiber cloth respectively;
[0026] Installing electric wires at both ends and the middle of the electrode, and performing welding processing on the contact position between the electric wire and the electrode;
[0027] The low freezing point sealing glue is applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer.
[0028] Furthermore, the preparation method of the conductive anti-icing coil material layer is as follows:
[0029] Pre-treat the carbon fiber cloth: prepare 3K carbon fiber cloth with a thickness of 0.1 to 0.5 mm, and dry it in a blast dryer at 100° C. for 8 hours;
[0030] Prepare two copper sheets with the dimensions of length × width × depth = 150 mm × 100 mm × 5 mm, and polish and grind their surfaces for use as electrodes;
[0031] Apply a conductive adhesive material to the inner side of the electrode (i.e., the side in contact with the carbon fiber cloth), fold the electrode in half along the wide side, sandwich the carbon fiber cloth between the two folded electrodes, compact them with a press, and install the two electrodes on both sides of the carbon fiber cloth respectively;
[0032] Install wires at both ends and the middle of the electrode, and perform welding on the contact position between the wire and the electrode;
[0033] The low freezing point sealing glue is evenly applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer, and the thickness of the conductive anti-icing coiled material layer is 0.1-0.5 mm.
[0034] The present invention also provides a method for preparing the self-melting ice ultra-thin wear layer material, comprising the following steps:
[0035] Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue;
[0036] The bonding glue is coated on one side of the conductive anti-icing coiled material layer, and after the bonding glue solidifies, a crushed stone rubber particle mixture is immediately laid and pressed into 2 to 4 mm, and after drying, excess crushed stone rubber particle mixture on the surface is removed to obtain an anti-skid and ice-breaking wear layer;
[0037] The hydrophobic ice-suppressing coating is laid on the surface of the anti-skid and ice-breaking wear layer to obtain a self-melting ice ultra-thin wear layer material.
[0038] Furthermore, the crushed stone rubber particle mixture is a mixture of rubber particles and black corundum crushed stone, and the mixing amount of the rubber particles is 3-8%.
[0039] Furthermore, the particle size of the rubber particles is 3 to 6 mm, and the particle size of the black corundum crushed stone is 3 to 5 mm.
[0040] The main function of the hydrophobic ice-suppressing coating in the self-melting ice ultra-thin wear layer material of the present invention is to reduce the adsorption capacity of thin ice on the road surface, to a certain extent inhibit the formation of thin ice on the road surface, and at the same time have the function of anti-skid road surface, and achieve the ice-suppressing effect after adding low freezing point materials. The main function of the anti-skid ice-breaking wear layer is to break ice and protect the road surface. By paving some elastic rubber particles on the road surface, the deformability of the rubber particles under pressure is utilized to make the road surface generate self-stress under load, so that the surface ice layer is broken, and the deicing ability of the road surface can be improved. When used, the mixed material pavement material produces a large compression deformation, which leads to a significant increase in the tensile stress and shear stress in the ice layer, causing the ice layer to break. Under the repeated action of the vehicle tires, the ice layer is destroyed, thereby overcoming the problems of the existing anti-freezing road paving materials that cannot effectively solve the problem of snow accumulation and ice on the road surface, and the shortcomings of poor road performance, low durability and large pollution. The main function of the conductive anti-icing coiled material layer of the present invention is to conduct heat. The present invention designs it as a coiled material design, which greatly improves the convenience of construction and reduces the difficulty of construction.
[0041] The present invention also provides application of the self-melting ice ultra-thin wear layer material in newly built road surfaces.
[0042] The present invention also provides application of the self-melting ice ultra-thin wear layer material in an existing road surface.
[0043] The self-melting ice ultra-thin wear layer material of the present invention is in the form of a coil, which will greatly reduce the construction difficulty in practical applications, broaden its application fields and usage scenarios, and is better suitable for special sections of highways, bridge decks and ramp areas.
[0044] When the self-melting ice ultra-thin wear layer material of the present invention is actually used, the conductive anti-icing coiled material layer is adhered to the road surface by adhesive glue.
[0045] The self-melting ultra-thin wear layer material of the present invention, as an active ice-melting method, needs to be laid on the road surface in advance. When thin ice forms on the road surface, it is electrified, and the conductive material carbon fiber cloth in the conductive anti-ice coil layer will generate heat by using its good conductivity, thereby achieving the ice-melting effect.
[0046] The self-melting ice ultra-thin wear layer of the present invention can not only melt snow and ice efficiently, but also has low construction difficulty and a wider application range.
[0047] Compared with the prior art, the present invention has the following advantages and technical effects:
[0048] (1) Enhanced anti-skid and hydrophobic performance: The surface hydrophobic and anti-icing coating can improve the hydrophobicity of the road surface, inhibit the formation of ice layers, reduce the adhesion of ice layers to the road surface, and further improve the durability and safety performance of the road surface.
[0049] (2) Improve de-icing efficiency: The combination of black corundum crushed stone and rubber particles in the anti-skid and ice-breaking wear layer can effectively break and melt the ice and snow on the road surface. The rubber particles, as elastic materials, have strong local deformation ability. Through the self-stress generated by the road surface under load, the ice and snow on the road surface are broken and melted, effectively inhibiting the icing of the road surface, thereby improving the de-icing efficiency of the road surface and enhancing the safety performance of the road.
[0050] (3) The conductive anti-icing coil layer is easy to construct: The carbon fiber cloth in the conductive anti-icing coil layer has good conductivity and can effectively generate heat to remove ice, allowing the road surface to quickly melt snow and ice, thereby improving the road's traffic capacity. Designed in the form of a coil, it is more conducive to practical application and construction. In addition, adding low-freezing point materials to the low-freezing point sealing glue can lower the freezing point of the road surface, making it less likely to freeze, and further improving the road surface's anti-icing performance.
[0051] (4) Lowering the freezing point of the road surface: By adding low-freezing-point materials to the hydrophobic anti-icing coating and low-freezing-point sealing glue, the freezing point of the road surface can be lowered, thereby achieving the effect of inhibiting the formation of ice on the road surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0053] Figure 1 This is a flow chart of the preparation of the self-melting ice ultra-thin wear layer material according to Example 1 of the present invention;
[0054] Figure 2 It is a top view of the electrode installation, where 1-copper sheet electrode, 2-carbon fiber cloth;
[0055] Figure 3 This is a three-dimensional diagram of electrode installation, where 1-copper sheet electrode, 2-carbon fiber cloth;
[0056] Figure 4 It is a schematic diagram of the structure of the self-melting ice ultra-thin wear layer material, wherein 4 is a hydrophobic ice-suppressing coating, 5 is an anti-skid ice-breaking wear layer, and 3 is a conductive anti-ice coil layer. DETAILED DESCRIPTION
[0057] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0058] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0059] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0060] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0061] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0062] Unless otherwise specified, the "normal temperature" in the embodiments of the present invention is 25±2°C.
[0063] All the raw materials used in the present invention are purchased from the market. For example, the silicone rubber solution is TP-3636# purchased from Jinhua Besilon Silicone Co., Ltd.; potassium carbonate is purchased from Shaoyuan Technology (Shanghai) Co., Ltd.; alkaline silica sol is JN-30 purchased from Sinopharm Chemical Reagent Co., Ltd.; methyl silicone oil is purchased from Aladdin Reagent (Shanghai) Co., Ltd.; SBS modified asphalt is purchased from Nanjing Tongli Construction Engineering Co., Ltd.; methyl silicate is purchased from Shanghai McLean Biochemical Technology Co., Ltd.; the accelerator is accelerator D, purchased from Haishun New Materials Co., Ltd.; the corrosion inhibitor is BTA corrosion inhibitor, purchased from Jinan Jinsheng New Materials Co., Ltd.; 3K carbon fiber cloth is purchased from Dezhou Junteng Materials Technology Co., Ltd.; urethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are all purchased from Sinopharm Chemical Reagent Co., Ltd.; PEG-2000 is purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; epoxy AB glue is purchased from Guangzhou Xiangxing Chemical Co., Ltd.
[0064] The technical solution of the present invention is further illustrated by the following embodiments.
[0065] Example 1
[0066] The preparation flow chart of the self-melting ice ultra-thin wear layer material of Example 1 of the present invention is shown in Figure 1 .
[0067] Preparation of conductive adhesive material: polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed in a mass ratio of 75:12:11:1.5:0.8, and stirred with a magnetic stirrer at a speed of 400 r / min for 30 min to obtain a conductive adhesive material for use.
[0068] Preparation of low freezing point sealing glue: polyurethane glue A (aqueous polyurethane resin purchased from Hangzhou Hemeng Chemical Co., Ltd.) and polyurethane glue B (trimethylolpropane, purchased from Shanghai Kaiyin Chemical Co., Ltd.) are mixed in a mass ratio of 9:4, and stirred at room temperature for 120s to obtain a two-component polyurethane glue, to which 5wt% sodium chloride (i.e., the amount of sodium chloride added is 5% of the total mass of the two-component polyurethane glue, the same below), 5wt% sodium acetate and 0.8wt% corrosion inhibitor (BTA corrosion inhibitor) are added to obtain a low freezing point polyurethane glue, and then 10wt% polyethylene glycol 2000 (PEG-2000) is added, and stirred evenly to obtain a low freezing point sealing glue for later use.
[0069] Preparation of a hydrophobic and ice-inhibiting coating: accurately weigh the following raw materials according to mass percentage: 10% silicone rubber solution (octamethylcyclotetrasiloxane), 10% potassium carbonate, 5% alkaline silica sol (JN-30), 0.5% methyl silicone oil, 1% SBS modified asphalt, 72.5% pure water, 0.8% methyl silicate and 0.2% accelerator (accelerator D), mix the above raw materials, stir at 400 r / min for 15 minutes to obtain a hydrophobic coating, add 4.5wt% sodium chloride (that is, the amount of sodium chloride added is 4.5% of the total mass of the above raw materials, the same below), 4.5wt% sodium acetate and 1wt% corrosion inhibitor, stir at 400 r / min for 5 minutes to prepare a hydrophobic and ice-inhibiting coating with a thickness of 0.3 mm, and set aside.
[0070] Preparation of conductive anti-icing coil layer:
[0071] (1) Pretreatment of carbon fiber cloth: Prepare 3K carbon fiber cloth with a thickness of 0.3 mm and dry it in a blast dryer at 100° C. for 8 h;
[0072] (2) Prepare two copper sheets with the dimensions of length × width × depth = 150 mm × 100 mm × 5 mm, polish and grind their surfaces, and use them as electrodes;
[0073] (3) Apply a conductive adhesive material (coating thickness 0.1-0.2 mm) to the inner side of the electrode (i.e., the side in contact with the carbon fiber cloth), fold the electrode in half along the wide side, sandwich the carbon fiber cloth between the two folded electrodes, compact them with a press, and install the two electrodes on both sides of the carbon fiber cloth respectively;
[0074] (4) Install wires at both ends and the middle of the electrode, and perform welding on the contact position between the wires and the electrode;
[0075] (5) low freezing point sealant glue is evenly applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer, the thickness of the conductive anti-icing coiled material layer is 0.3 mm, and it is set aside.
[0076] The top view of electrode installation is shown in Figure 2 , where 1-copper sheet electrode, 2-carbon fiber cloth; see the three-dimensional diagram of electrode laying Figure 3 , where 1-copper sheet electrode, 2-carbon fiber cloth.
[0077] Preparation of self-melting ice ultra-thin wear layer material:
[0078] Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue;
[0079] Adhesive glue is applied to one side of the conductive anti-icing coiled material layer. After the adhesive glue solidifies, a crushed stone rubber particle mixture is immediately laid and pressed into 3 mm. After drying, excess crushed stone rubber particle mixture on the surface is removed to obtain an anti-skid and ice-breaking wear layer with a thickness of 3 mm. In this embodiment, the crushed stone rubber particle mixture is a mixture of rubber particles with a particle size of 3 to 6 mm and black corundum crushed stones with a particle size of 3 to 5 mm, and the amount of rubber particles is 5%;
[0080] The hydrophobic ice-suppressing coating is evenly laid on the surface of the anti-skid ice-breaking wear layer (i.e., the hydrophobic ice-suppressing coating is directly coated on the surface of the anti-skid ice-breaking wear layer), and a self-melting ice ultra-thin wear layer material is obtained. The structural schematic diagram of the self-melting ice ultra-thin wear layer material is shown in Figure 4 , among which 4 is a hydrophobic anti-icing coating, 5 is an anti-skid and ice-breaking wear layer, and 3 is a conductive anti-icing coil layer.
[0081] Example 2
[0082] Preparation of conductive adhesive material: polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed in a mass ratio of 75:10:12:1:0.5, and stirred with a magnetic stirrer at a speed of 400 r / min for 30 min to obtain a conductive adhesive material for use.
[0083] Preparation of low freezing point sealing glue: polyurethane glue A (water-based polyurethane resin, purchased from Hangzhou Hemeng Chemical Co., Ltd.) and polyurethane glue B (trimethylolpropane, purchased from Shanghai Kaiyin Chemical Co., Ltd.) are mixed in a mass ratio of 4:5, stirred at room temperature for 120s to obtain a two-component polyurethane glue, 4wt% sodium chloride, 6wt% sodium acetate and 0.5wt% corrosion inhibitor (BTA corrosion inhibitor) are added thereto to obtain a low freezing point polyurethane glue, and then 12wt% PEG-2000 is added and stirred evenly to obtain a low freezing point sealing glue for later use.
[0084] Preparation of a hydrophobic and anti-icing coating: accurately weigh the following raw materials according to their mass percentage: 15% silicone rubber solution (octamethylcyclotetrasiloxane), 8% potassium carbonate, 3% alkaline silica sol (colloid silica solution), 1% methyl silicone oil, 1.5% SBS modified asphalt, 70.7% pure water, 0.5% methyl silicate and 0.3% accelerator (accelerator D), mix the above raw materials, stir at 400 r / min for 15 min to obtain a hydrophobic coating, add 4wt% sodium chloride, 4wt% sodium acetate and 0.5wt% corrosion inhibitor to prepare a hydrophobic and anti-icing coating with a thickness of 0.1 mm, and set aside.
[0085] Preparation of conductive anti-icing coil layer:
[0086] (1) Pretreatment of the carbon fiber cloth: prepare a 3K carbon fiber cloth with a thickness of 0.1 mm and dry it in a blast dryer at 100° C. for 8 h;
[0087] (2) Prepare two copper sheets with the dimensions of length × width × depth = 150 mm × 100 mm × 5 mm, polish and grind their surfaces, and use them as electrodes;
[0088] (3) Apply a conductive adhesive material to the inner side of the electrode (i.e., the side in contact with the carbon fiber cloth), fold the electrode in half along the wide side, sandwich the carbon fiber cloth between the two folded electrodes, compact them with a press, and install the two electrodes on both sides of the carbon fiber cloth respectively;
[0089] (4) Install wires at both ends and the middle of the electrode, and perform welding on the contact position between the wires and the electrode;
[0090] (5) low freezing point sealant glue is evenly applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer, the thickness of the conductive anti-icing coiled material layer is 0.1 mm, and it is set aside.
[0091] Preparation of self-melting ice ultra-thin wear layer material:
[0092] Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue;
[0093] Adhesive glue is applied to one side of the conductive anti-icing coiled material layer. After the adhesive glue solidifies, a crushed stone rubber particle mixture is immediately laid and pressed into 4 mm. After drying, excess crushed stone rubber particle mixture on the surface is removed to obtain an anti-skid and ice-breaking wear layer with a thickness of 4.5 mm. In this embodiment, the crushed stone rubber particle mixture is a mixture of rubber particles with a particle size of 3 to 6 mm and black corundum crushed stones with a particle size of 3 to 5 mm, and the mixing amount of rubber particles is 8%;
[0094] The hydrophobic ice-suppressing coating is evenly laid on the surface of the anti-skid and ice-breaking wear layer to obtain a self-melting ice ultra-thin wear layer material.
[0095] Example 3
[0096] Preparation of conductive adhesive material: polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed in a mass ratio of 75:15:10:2:1, and stirred with a magnetic stirrer at a speed of 400 r / min for 30 min to obtain a conductive adhesive material for use.
[0097] Preparation of low freezing point sealing glue: polyurethane glue A (water-based polyurethane resin, purchased from Hangzhou Hemeng Chemical Co., Ltd.) and polyurethane glue B (trimethylolpropane, purchased from Shanghai Kaiyin Chemical Co., Ltd.) are mixed in a mass ratio of 8:3, stirred at room temperature for 120s to obtain a two-component polyurethane glue, 6wt% sodium chloride, 4wt% sodium acetate and 1wt% corrosion inhibitor (BTA corrosion inhibitor) are added thereto to obtain a low freezing point polyurethane glue, and then 10wt% PEG-2000 is added and stirred evenly to obtain a low freezing point sealing glue for later use.
[0098] Preparation of a hydrophobic and anti-icing coating: accurately weigh the following raw materials according to their mass percentage: 8% silicone rubber solution (octamethylcyclotetrasiloxane), 11% potassium carbonate, 8% alkaline silica sol (colloid silica solution), 0.5% methyl silicone oil, 0.8% SBS modified asphalt, 70.8% pure water, 0.8% methyl silicate and 0.1% accelerator (accelerator D), mix the above raw materials, stir at 400 r / min for 15 minutes to obtain a hydrophobic coating, add 6wt% sodium chloride, 6wt% sodium acetate and 1wt% corrosion inhibitor to prepare a hydrophobic and anti-icing coating with a thickness of 0.5 mm, and set aside.
[0099] Preparation of conductive anti-icing coil layer:
[0100] (1) Pretreatment of the carbon fiber cloth: prepare a 3K carbon fiber cloth with a thickness of 0.5 mm and dry it in a blast dryer at 100° C. for 8 h;
[0101] (2) Prepare two copper sheets with the dimensions of length × width × depth = 150 mm × 100 mm × 5 mm, polish and grind their surfaces, and use them as electrodes;
[0102] (3) Apply a conductive adhesive material to the inner side of the electrode (i.e., the side in contact with the carbon fiber cloth), fold the electrode in half along the wide side, sandwich the carbon fiber cloth between the two folded electrodes, compact them with a press, and install the two electrodes on both sides of the carbon fiber cloth respectively;
[0103] (4) Install wires at both ends and the middle of the electrode, and perform welding on the contact position between the wires and the electrode;
[0104] (5) low freezing point sealant glue is evenly applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer, the thickness of the conductive anti-icing coiled material layer is 0.5 mm, and it is set aside.
[0105] Preparation of self-melting ice ultra-thin wear layer material:
[0106] Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue;
[0107] Adhesive glue is applied to one side of the conductive anti-icing coiled material layer. After the adhesive glue solidifies, a crushed stone rubber particle mixture is immediately laid and pressed into 4 mm. After drying, excess crushed stone rubber particle mixture on the surface is removed to obtain an anti-skid and ice-breaking wear layer with a thickness of 6 mm. In this embodiment, the crushed stone rubber particle mixture is a mixture of rubber particles with a particle size of 3 to 6 mm and black corundum crushed stone with a particle size of 3 to 5 mm, and the mixing amount of rubber particles is 3%;
[0108] The hydrophobic ice-suppressing coating is evenly laid on the surface of the anti-skid and ice-breaking wear layer to obtain a self-melting ice ultra-thin wear layer material.
[0109] Comparative Example 1
[0110] The same as Example 1, except that no low freezing point material (sodium chloride and sodium acetate) and corrosion inhibitor are added when preparing the low freezing point seal glue and the hydrophobic ice-inhibiting coating.
[0111] Comparative Example 2
[0112] The same as Example 1, except that the self-melting ice ultra-thin wear layer material does not contain a hydrophobic ice-suppressing coating.
[0113] Comparative Example 3
[0114] The same as Example 1, except that the carbon fiber cloth is not introduced in the preparation of the conductive anti-icing coiled material layer, that is, when preparing the conductive anti-icing coiled material layer, the conductive heating material carbon fiber cloth is replaced with a mixture of graphite (purchased from Shanghai Yifan Graphite Co., Ltd.) and carbon fiber (purchased from Shenzhen Carbonene Technology Co., Ltd.) (the mass ratio of the two is 1:1), and the specific steps are as follows:
[0115] Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue;
[0116] Preparation of conductive mixture: Select 2mm long chopped carbon fiber, prepare conductive mixture according to the ratio of 25wt% graphite (accounting for the proportion of the whole conductive mixture) and 4wt% chopped carbon fiber (accounting for the proportion of the whole conductive mixture), add chopped carbon fiber and graphite into adhesive glue and stir continuously until the conductive component and adhesive glue are evenly mixed.
[0117] In order to better verify the experimental effect of the present invention, the following experiment was designed.
[0118] After laying according to the above method, the self-melting ice ultra-thin wear layer materials of Example 1 and Comparative Example 3 were subjected to a conductivity test. The specific method is: after power is turned on, different voltage values are set, the current flowing through the material is measured, and the final conductivity is calculated using Ohm's law. The conductivity test results are shown in Table 1.
[0119] Table 1 Conductivity measurement results
[0120] Voltage (V) Example 1 Conductivity (S / m) Comparative Example 3 Conductivity (S / m) 5.0 1.5 1.3 10.0 1.8 1.7 15.0 2.4 2.2 20.0 2.6 2.3 25.0 2.7 2.6 30.0 2.9 2.7 35.0 3.2 3.0
[0121] As can be seen from Table 1, the self-melting ice ultra-thin wear layer prepared in Example 1 of the present invention is superior to the wear layer composed of other conductive materials in terms of conductivity. This is because the carbon fibers in the carbon fiber cloth are arranged in a certain direction. This arrangement structure is conducive to the conduction of electrons in the material, thereby improving the conductivity, and the surface of the carbon fiber is specially treated, with higher conductivity and better conductivity. In contrast, the graphite particles and carbon fibers in the graphite carbon fiber mixture have uneven particle sizes, local agglomeration, or unsatisfactory surface conditions, and have poor conductivity.
[0122] At an input power of 150W / m 2 When the same mass of water is poured on the self-melting ultra-thin wear layer materials of Example 1 and Comparative Examples 1 to 3, the water and the plate are frozen to form 5 mm thin ice. The freezing temperature is tested, and the results are shown in Table 2.
[0123] Table 2 Freezing temperature measurement results
[0124] Freezing temperature(℃) Example 1 -15.0 Comparative Example 1 -5.0 Comparative Example 2 -1.0 Comparative Example 3 -1.0
[0125] As can be seen from Table 2, by adding low freezing point materials to the glue and the hydrophobic ice-suppressing coating, the freezing temperature of the overall wear layer of Example 1 is greatly reduced, which is far better than that of the comparative examples. This is because when sodium chloride or sodium acetate is dissolved in the glue, their ions will interact with the water molecules in the glue to form ionized glue. The interaction between these ions and water molecules will interfere with the crystallization process of the water molecules and hinder the formation of ice crystals.
[0126] The ice melting experiment was conducted on the self-melting ultra-thin wear layer materials of Example 1 and Comparative Examples 1 to 3. The surface temperature of the self-melting ultra-thin wear layer materials of Example 1 and Comparative Examples 1 to 3 was recorded every 15 minutes. When the temperature was continuously higher than 0°C (the ice was completely melted), the temperature recording was stopped. The input power was 150W / m 2 , air temperature is -5℃, and thin ice thickness is 5mm. The experimental results of ice melting time are shown in Table 3.
[0127] Table 3 De-ice time measurement results
[0128]
[0129] From the experimental results, it can be seen that the ice melting time of Example 1 is shorter and the ice melting effect is better. By comparing Example 1 with Comparative Example 3, it can be seen that the conductive heating effect of the carbon fiber cloth is better than that of the graphite and carbon fiber mixture, and has a better ice melting effect and ice melting ability.
[0130] The road performance of the self-melting ultra-thin wear layer material of Example 1 was tested. The self-melting ultra-thin wear layer material of Example 1 was spread in the test tank of the MMLS3 small accelerated loading equipment and an accelerated loading experiment was carried out. The swing value (BPN) of the self-melting ultra-thin wear layer was tested by loading it to a certain number of times. The results are shown in Table 4.
[0131] Table 4 Measurement of swing values (BPN) under different wheel load times
[0132]
[0133] It can be seen from the experimental results that with the increase of wheel load times, the swing value decreases, but the swing value can be maintained above 61BPN, indicating that the self-melting ice ultra-thin wear layer has good anti-skid performance and anti-skid durability, and after the loading is completed, the self-melting ice ultra-thin wear layer material does not show obvious rutting and gravel falling off, indicating that it has good rutting resistance. It can be seen that the self-melting ice ultra-thin wear layer material has good road performance.
[0134] In summary, the present invention aims at the road surface ice-melting technology and introduces a self-melting ultra-thin wear layer material, which has a simple production process and low application and construction difficulty. It not only meets the basic road performance but also has a good ice-melting effect.
[0135] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A self-melting ice ultra-thin wear layer material, characterized in that: It is composed of a hydrophobic ice-suppressing coating, an anti-skid and ice-breaking wear layer, and a conductive anti-icing coil layer; The anti-skid and ice-breaking wear layer is located between the hydrophobic ice-suppressing coating and the conductive anti-icing coiled material layer; The preparation method of the conductive anti-icing coil material layer is as follows: Drying the carbon fiber cloth; The surfaces of two copper sheets are polished and ground to serve as electrodes; Applying a conductive adhesive material on the inner side of the electrode, folding the electrode in half along the wide side, sandwiching the dried carbon fiber cloth between the two folded electrodes, compacting, and installing the two electrodes on both sides of the carbon fiber cloth respectively; Installing electric wires at both ends and the middle of the electrode, and performing welding processing on the contact position between the electric wire and the electrode; The low freezing point sealing glue is applied to the upper and lower surfaces of the carbon fiber cloth to form a conductive anti-icing coiled material layer.
2. The self-melting ice ultra-thin wear layer material according to claim 1, characterized in that: The thickness of the hydrophobic ice-suppressing coating is 0.1 to 0.5 mm, the thickness of the anti-skid and ice-breaking wear layer is 3 to 6 mm, and the thickness of the conductive anti-ice coil layer is 0.1 to 0.5 mm.
3. The self-melting ice ultra-thin wear layer material according to claim 1, characterized in that: The hydrophobic ice-inhibiting coating comprises the following raw materials, measured by mass percentage: 8-15% silicone rubber solution, 8-15% potassium carbonate, 3-8% alkaline silica sol, 0.5-1% methyl silicone oil, 0.8-1.5% SBS modified asphalt, 70-80% water, 0.5-0.8% methyl silicate and 0.1-0.3% accelerator.
4. The self-melting ice ultra-thin wear layer material according to claim 3, characterized in that: The preparation method of the hydrophobic anti-icing coating is as follows: accurately weigh each raw material according to the mass percentage, mix and stir evenly to obtain a hydrophobic coating raw material mixture, add sodium chloride, sodium acetate and a corrosion inhibitor to the hydrophobic coating raw material mixture, and obtain the hydrophobic anti-icing coating after coating.
5. The self-melting ice ultra-thin wear layer material according to claim 1, characterized in that: The raw materials of the conductive anti-icing coiled material layer include: carbon fiber cloth, copper sheet, conductive adhesive material and low freezing point sealing glue.
6. The self-melting ice ultra-thin wear layer material according to claim 5, characterized in that: The preparation method of the conductive adhesive material is as follows: polyurethane acrylate, lauryl methacrylate, isocyanate, tert-butyl perbenzoate and epoxy phosphate are mixed in a mass ratio of 75: (10-15): (10-12): (1-2): (0.5-1) to obtain the conductive adhesive material; The preparation method of the low freezing point sealant glue is as follows: adding a low freezing point material and a corrosion inhibitor into a two-component polyurethane glue to obtain a low freezing point polyurethane glue, and then adding polyethylene glycol, mixing evenly, to obtain the low freezing point sealant glue.
7. A method for preparing the self-melting ice ultra-thin wear layer material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mix glue A and glue B of epoxy AB glue in a mass ratio of 2:1 to form a bonding glue; The bonding glue is coated on one side of the conductive anti-icing coiled material layer, and after the bonding glue solidifies, a crushed stone rubber particle mixture is immediately laid and pressed into 2 to 4 mm, and after drying, excess crushed stone rubber particle mixture on the surface is removed to obtain an anti-skid and ice-breaking wear layer; The hydrophobic ice-suppressing coating is laid on the surface of the anti-skid and ice-breaking wear layer to obtain a self-melting ice ultra-thin wear layer material.
8. Use of the self-melting ice ultra-thin wear layer material according to any one of claims 1 to 6 in newly built pavement.
9. Use of the self-melting ice ultra-thin wear layer material according to any one of claims 1 to 6 in an existing road surface.
Citation Information
Patent Citations
Method for preparing polyurethane rubber granule mixture for pavement self-stress icebreaking
CN103058585A
Electric-conduction anti-skid wearing layer for pavement and preparation method thereof
CN105256694A
Anti-freezing slow-release coating process
CN116200076A