Dual-wavelength aggregation-induced luminescence magnetically encoded microspheres and preparation method and application thereof
By using dual-wavelength aggregation-induced luminescence magnetically encoded microspheres in in vitro diagnostic technology, using active swelling method and in situ precipitation method, the problem of fluorescence quenching of traditional fluorescent materials in aggregation state is solved, and high encoding capacity and stability are achieved AIE magnetically encoded microspheres are suitable for coding applications of 24 and above.
Patent Information
- Application Number
- CN202410144972.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-02-01
AI Technical Summary
In the prior art, traditional fluorescent materials experience fluorescence quenching in aggregation state, which limits the encoding capacity and stability, and the encoding capability of quantum dot-encoded microspheres is limited by the reabsorption and color-sequential effects between fluorescent signals.
Double-wavelength aggregation-induced luminescence (AIE) magnetically encoded microspheres are adopted to embed AIE molecules inside blank polymer microspheres by active swelling method, and magnetic particles are deposited on the surface of the microspheres by in-situ precipitation method to achieve high coding capacity and stability sex.
Dual-wavelength AIE magnetically encoded microspheres with high encoding capacity, no string color effect and fluorescence intensity can achieve encoding capacity of 24 weights and above, and improve detection stability.
Smart Images

Figure CN118033124B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of in vitro diagnosis, and in particular relates to a dual-wavelength aggregation-induced luminescence magnetically encoded microsphere and a preparation method and application thereof. Background Art
[0002] The development and completion of the human genome and proteome in recent years has led to a huge demand for large-scale analysis of biomolecules, which has promoted the rapid development of liquid suspension biochips with encoded microspheres as the core. Liquid suspension biochips with rapid high-throughput flow cytometry and magnetic separation as analytical methods have gradually become a new goal for accurate diagnosis by performing rapid and high-throughput multiplex detection of markers such as proteins, nucleic acids and small molecules. Among them, the development of encoded microspheres with high encoding capacity and stability is still a huge challenge. The design of suitable encoded microspheres has the following requirements: high photostability, good anti-magnetism, large number of codes, no reabsorption and crosstalk effects, etc.
[0003] Spectral signals are widely used in the construction of liquid biochips due to their flexible encoding and fast decoding speed. At present, the commonly used spectral encoding materials are mainly organic materials, quantum dots, upconversion dots and photonic crystals, etc. Quantum dots have become popular encoding materials due to their high brightness and narrow emission spectrum, but the encoding ability of quantum dots is limited by the reabsorption and cross-color effect between quantum dot fluorescence signals, which limits the application of quantum dot encoding microspheres.
[0004] At present, commercial liquid biochip Luminex system and BD's cytometric bead array all use organic dyes for encoding, but traditional organic materials have fluorescence quenching in the aggregated state, which limits the encoding capacity and stability of traditional organic materials. The new aggregation-induced emission (AIE) material discovered by the team of Academician Tang Benzhong in 2001 is a promising encoding material for the preparation of encoded microspheres, because AIE materials can achieve in-situ enhancement of fluorescence signals during the aggregation process. Aggregation-induced emission materials have properties such as large Stokes shift, strong resistance to photobleaching, and anti-magnetism, and are an excellent encoding microsphere material. However, there are few public reports on the efficient preparation of magnetic fluorescence encoding using AIE materials. Therefore, it is very necessary to develop a technology for the efficient and direct generation of aggregation-induced emission magnetic encoded microspheres. Summary of the invention
[0005] In order to solve the shortcomings of the prior art, the present invention aims to provide a dual-wavelength aggregation-induced luminescence magnetically encoded microsphere and a preparation method and application thereof. The prepared dual-wavelength aggregation-induced luminescence magnetically encoded microsphere has the characteristics of high coding capacity, no cross-color effect and high fluorescence intensity.
[0006] The technical solution adopted by the present invention is:
[0007] A dual-wavelength aggregation-induced luminescence magnetically encoded microsphere, comprising an AIE polymer microsphere and magnetic particles; the AIE polymer microsphere is obtained by embedding an AIE molecule inside a blank polymer microsphere, and the magnetic particles are deposited on the surface of the AIE polymer microsphere; the AIE molecule comprises an AIE-R molecule and an AIE-IR molecule;
[0008] The difference between the maximum emission wavelength of the AIE-IR molecule and the maximum emission wavelength of the AIE-R molecule is in the range of 160 nm to 290 nm, and satisfies Δλ≥185. Among them, I / I 0 is the average value of the ratio of the fluorescence intensity of the AIE-IR molecule and the AIE-IR molecule before and after embedding, λ IR is the maximum emission wavelength of the AIE-IR molecule, λ R is the maximum emission wavelength of the AIE-R molecule.
[0009] Preferably, the blank polymer microspheres are selected from at least one of polystyrene microspheres, polymethyl methacrylate microspheres and polyglycidyl acrylate microspheres;
[0010] Further preferably, the blank polymer microspheres are selected from polystyrene microspheres or polyglycidyl acrylate microspheres.
[0011] Preferably, the magnetic particles are Fe 3 O 4 ;
[0012] Preferably, the AIE-R molecule is selected from at least one of the following AIE-R1 to AIE-R16 molecules:
[0013]
[0014]
[0015] Alkyl chain in AIE-R 1 molecule -C 8 H 17 Each is independently a branched chain alkyl or a straight chain alkyl.
[0016] Alkyl chain in AIE-R 11 molecule -C 6 H 13 Each is independently a branched chain alkyl or a straight chain alkyl.
[0017] The AIE-IR molecule is selected from at least one of the following AIE-IR1 to AIE-IR10 molecules:
[0018]
[0019]
[0020] Preferably, the AIE molecules are embedded in the blank polymer microspheres by an active swelling method, wherein the amount of the AIE molecules used in the active swelling method is 0.01-10wt% of the amount of the blank polymer microspheres, wherein the mass amount of the AIE-R molecules accounts for 0.01% to 1000% of the mass amount of the AIE-IR molecules;
[0021] Further preferably, the active swelling method is to allow the AIE molecules to swell with the blank polymer microspheres via a swelling agent so that the AIE molecules are embedded inside the blank polymer microspheres;
[0022] More preferably, in the active swelling method, the swelling agent is selected from at least one of dichloromethane, tetrahydrofuran, chloroform, anisole, benzyl alcohol and toluene, and the particle size of the blank polymer microspheres ranges from 0.03 μm to 50 μm;
[0023] More preferably, the particle size of the blank polymer microspheres ranges from 0.5 μm to 10 μm.
[0024] Preferably, the magnetic particles are deposited on the surface of the AIE polymer microspheres by an in-situ precipitation method of iron salts, wherein the amount of iron salts used in the in-situ precipitation method is 0.1-25 wt % of the amount of blank polymer microspheres used.
[0025] Further preferably, the in-situ precipitation method is to add an alkaline solution to react with the iron salt chelated on the surface of the AIE polymer microspheres in situ to generate magnetic particles that are deposited on the surface of the AIE polymer microspheres.
[0026] More preferably, in the in-situ precipitation method, the surface of the AIE polymer microspheres is modified by sulfonation, the alkaline solution is selected from at least one of sodium hydroxide solution, ammonia water, potassium hydroxide solution and sodium bicarbonate solution; the iron salt is selected from at least one of a trivalent iron salt and a divalent iron salt; the trivalent iron salt is selected from at least one of ferric chloride hexahydrate and anhydrous ferric chloride; the divalent iron salt is selected from at least one of ferrous chloride tetrahydrate, ferrous chloride dihydrate, ferrous sulfate and ferrous sulfate heptahydrate.
[0027] More preferably, considering the uniformity of magnetic particles deposited on the surface of the AIE polymer microspheres, the iron salt is a compound of a trivalent iron salt and a divalent iron salt, wherein the mass amount of the trivalent iron salt is 10% to 60% of the mass amount of the divalent iron salt.
[0028] Preferably, the encoding capacity of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres is ≥24, and the CV value of the flow fluorescence signal and the CV value of the flow FCS are both less than 10%.
[0029] The preparation method of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres comprises the following steps:
[0030] S1. Preparation of AIE polymer microspheres by active swelling method
[0031] (1) dispersing blank polymer microspheres in water to obtain a microsphere dispersion;
[0032] (2) dissolving the AIE molecules in a swelling agent to obtain an AIE swelling agent solution;
[0033] (3) adding the AIE swelling agent solution described in step (2) to the microsphere dispersion described in step (1), and after ultrasonic treatment, closing the reactor to carry out swelling reaction. After the reaction is completed, volatilizing and removing the swelling agent to obtain AIE polymer microspheres;
[0034] S2. Preparation of dual-wavelength aggregation-induced luminescence magnetically encoded microspheres by in situ precipitation
[0035] The AIE polymer microspheres of step S1 are dissolved in a sulfuric acid solution, the temperature is increased for reaction, and the supernatant is removed by centrifugation to obtain AIE polymer microspheres with sulfonation-modified surfaces. The AIE polymer microspheres are mixed with iron salt and water for reaction, and the supernatant is removed by centrifugation to obtain iron salt-chelated AIE polymer microspheres. An alkaline solution is added, and the temperature is increased. The iron salt reacts in situ to generate magnetic particles that are deposited on the surface of the AIE polymer microspheres. The supernatant is removed by centrifugation to prepare dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
[0036] Preferably, the preparation method of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres comprises the following steps:
[0037] S1. Preparation of AIE polymer microspheres by active swelling method
[0038] (1) dispersing blank polymer microspheres in water to obtain a microsphere dispersion;
[0039] (2) dissolving the AIE molecules in a swelling agent to obtain an AIE swelling agent solution;
[0040] (3) adding the AIE swelling agent solution described in step (2) to the microsphere dispersion described in step (1), and after ultrasonic treatment at an ultrasonic power of 50 W to 400 W for 1 min to 30 min, a closed reactor is used for swelling reaction for 0.5 h to 4 h. After the reaction is completed, the swelling agent is volatilized to obtain AIE polymer microspheres;
[0041] S2. Preparation of dual-wavelength aggregation-induced luminescence magnetically encoded microspheres by in situ precipitation
[0042] The AIE polymer microspheres of step S1 are dissolved in a sulfuric acid solution, the temperature is raised to 30°C to 100°C and the reaction is carried out for 4h to 12h, and the supernatant is removed by centrifugation to obtain AIE polymer microspheres with sulfonation modified on the surface. The microspheres are mixed with iron salt and water, and the mixture is immersed in the solution for reaction for 0.5h to 10h, and the supernatant is removed by centrifugation to obtain iron salt chelated AIE polymer microspheres. An alkaline solution is added, and the temperature is raised to 60°C to 120°C and the reaction is carried out for 0.5h to 4h. The iron salt reacts in situ to generate magnetic particles which are deposited on the surface of the AIE polymer microspheres. The supernatant is removed by centrifugation to prepare dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
[0043] Further preferably, in step S1, the ultrasonic power of step (3) is 300W, the ultrasonic treatment time is 5 minutes, and the time for volatilizing and removing the swelling agent is 2 hours to 10 hours. More preferably, the time for volatilizing and removing the swelling agent is 4 hours.
[0044] Further preferably, in step S2, the soaking reaction time is 2 h to 4 h.
[0045] Preferably, in step S1, the mass amount of blank polymer microspheres in the microsphere dispersion is 0.1% to 20% of the mass amount of water;
[0046] Further preferably, the mass amount of blank polymer microspheres in the microsphere dispersion is 0.5% to 10% of the mass amount of water.
[0047] Preferably, in step S1, the mass amount of the AIE molecules in the AIE swelling agent solution is 0.1% to 50% of the mass amount of the swelling agent;
[0048] Preferably, in step S2, the mass concentration of the sulfuric acid solution is 70% to 99%; the mass amount of the AIE polymer microspheres is 1% to 30% of the mass amount of the sulfuric acid solution;
[0049] Further preferably, the mass concentration of the sulfuric acid solution is 98.3%; and the mass amount of the AIE polymer microspheres is 5% to 20% of the mass amount of the sulfuric acid solution.
[0050] Preferably, in step S2, the mass dosage of the iron salt is 0.0005% to 25% of the mass dosage of water; the mass dosage of the alkaline solution is 0.1% to 50% of the mass dosage of water; the mass concentration of the alkaline solution is 1% to 10%;
[0051] Preferably, the water in step S1 and step S2 is ultrapure water; the centrifugal speed is 3000 rpm to 6000 rpm, the centrifugal time is 5 min to 60 min, and the number of centrifugation is more than three times.
[0052] The above-mentioned dual-wavelength aggregation-induced luminescence magnetically encoded microspheres are used in in vitro non-disease diagnostic testing.
[0053] The present invention proposes a new technology for efficiently preparing dual-wavelength aggregation-induced emission (AIE) magnetically encoded microspheres by combining active swelling and in-situ generation. Two AIE molecules of different wavelengths are actively swollen into the interior of the microsphere matrix through hydrophobic interaction and concentration difference, and magnetic particles are generated on the surface of the microspheres by the in-situ generation method of iron salts. At the same time, by selecting two AIE molecules of different wavelengths, dual-wavelength aggregation-induced emission magnetically encoded microspheres with uniform particle size and high encoding capacity are obtained. The microspheres have excellent detection stability and can achieve 24 or more encodings.
[0054] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in:
[0055] (1) Compared with the fluorescent materials of traditional magnetically encoded microspheres, the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres of the present invention use AIE materials to improve the encoding capacity of magnetically encoded microspheres and solve the problem of fluorescence reabsorption effect of traditional fluorescent materials inside the microspheres. Even in microspheres with high magnetic content, the dual-wavelength AIE encoding capacity can reach 24-fold capacity.
[0056] (2) The present invention uses a simple swelling volatilization and in-situ generation technology to encapsulate high-concentration dual-wavelength AIE molecules inside the microspheres, and deposits magnetic particles in situ on the surface of the microspheres. By adjusting the content of AIE molecules of different wavelengths and the mass content of iron salts, AIE magnetic fluorescent encoded microspheres with optimal performance are obtained.
[0057] (3) Generally speaking, traditional fluorescent materials will have fluorescence attenuation in the FRET process. Since the dipole moment interaction between the two AIE molecules is greater than the FRET process, the two different AIE molecules in the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres of the present invention have a fluorescence enhancement effect inside the microspheres. At the same time, the AIE material has typical aggregation-induced luminescence properties. The two different AIE molecules are embedded in the microspheres and can emit strong fluorescence in the aggregate.
[0058] (4) The preparation method of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres of the present invention is simple. The synergistic effect of the aggregation-induced luminescence of AIE molecules and the intermolecular dipole moment effect is utilized to obtain dual-wavelength AIE magnetically encoded microspheres with high encoding capacity, thereby realizing the effective application of AIE molecules in the preparation of encoded microspheres, adding an important fluorescent material to the encoding elements, and providing a new encoding strategy for the core raw materials of protein biochips. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 This is a scanning electron microscope image of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres prepared in Example 1.
[0060] Figure 2 This is the emission spectra of AIE-R1 and AIE-IR1 in the dual-wavelength aggregation-induced emission magnetically encoded microspheres prepared in Example 1.
[0061] Figure 3 Schematic diagram of flow encoding of dual-wavelength aggregation-induced luminescence magnetic encoding microspheres prepared in Example 1. DETAILED DESCRIPTION
[0062] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0063] The blank polymer microspheres in the examples and comparative examples are polystyrene polymer microspheres with a diameter of 5 μm, which are from AIE Research Institute and have a product number of NWKPB-500.
[0064] Example 1
[0065] Weigh 1 g of blank polymer microspheres and disperse them in 100 g of water to obtain a microsphere dispersion;
[0066] 5 mg of AIE-R1 molecules (alkyl chain-C 8 H 17 The AIE polymer microspheres were prepared by mixing the two solutions (the total mass of AIE molecules accounted for 1 wt% of the mass of the blank polymer microspheres) and ultrasonically treating them at a power of 100 W for 1 min. After the closed swelling for 2 h, the solvent was evaporated for 4 h, and the supernatant was removed by centrifugation to obtain the AIE polymer microspheres. The obtained AIE polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h. The microspheres were centrifuged at 5000 rpm and resuspended in water. The reaction was repeated three times to obtain the AIE polymer microspheres with sulfonated surface.
[0067] Ferrous sulfate heptahydrate and ferric chloride hexahydrate were mixed with 100g water in a mass ratio of 2:1 (the total mass of iron salt accounted for 5wt% of the mass of blank polymer microspheres), and the AIE polymer microspheres with sulfonation modified on the surface obtained above were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 50mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80℃, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
[0068] The morphology of dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was observed using a field emission SEM electron microscope. The microspheres showed a regular spherical structure with a statistical particle size of about 5 μm (e.g. Figure 1 The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R1 was 620nm, and the ratio of the fluorescence intensity of AIE-R1 before and after coating was 1300. The emission wavelength of AIE-IR1 was 780nm, and the ratio of the fluorescence intensity of AIE-IR1 before and after coating was 1200. The difference in the central wavelength was 160nm (such as Figure 2 ). The encoding data of dual-wavelength aggregation-induced luminescence magnetic encoded microspheres were tested using an analytical flow cytometer. The CV value of the flow fluorescence signal tested was 4.6%, the CV value of the flow FCS was 5.7%, and the encoding peak was 24 (such as Figure 3 ), encoding is successful.
[0069] Comparative Example 1
[0070] Weigh 1 g of blank polymer microspheres and disperse them in 100 g of water to obtain a microsphere dispersion;
[0071] 5 mg of AIE-R4 molecules and 5 mg of AIE-IR1 molecules were dissolved in 10 mL of tetrahydrofuran to obtain an AIE swelling agent solution; the two solutions were mixed together (the total mass of AIE molecules accounted for 1 wt% of the mass of blank polymer microspheres), and ultrasonically treated at a power of 100 W for 1 min. After the closed swelling for 2 h, the solvent was evaporated for 4 h, and the supernatant was removed by centrifugation to obtain AIE polymer microspheres. The obtained AIE polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at 5000 rpm, and then resuspended in water, and repeated three times to obtain AIE polymer microspheres with sulfonated surface modification.
[0072] Ferrous sulfate heptahydrate and ferric chloride hexahydrate were mixed with 100g water in a mass ratio of 2:1 (the total mass of iron salt accounted for 5wt% of the mass of blank polymer microspheres), and the AIE polymer microspheres with sulfonation modified on the surface obtained above were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 50mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80℃, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
[0073] The morphology of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was observed using a field emission SEM electron microscope. The microspheres showed a regular spherical structure with a statistical particle size of about 5μm. The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R4 was 650nm, and the ratio of the fluorescence intensity before and after the coating of AIE-R4 was 1200. The emission wavelength of AIE-IR1 was 780nm, and the ratio of the fluorescence intensity before and after the coating of AIE-IR1 was 1300. The difference in central wavelength was 130nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal tested was 14.6%, and the CV value of the flow FCS was 25.7%, indicating that the encoding failed.
[0074] Comparative Example 2
[0075] Weigh 1 g of blank polymer microspheres and disperse them in 100 g of water to obtain a microsphere dispersion;
[0076] 5 mg of AIE-R1 molecules (alkyl chain-C 8 H 17 The AIE polymer microspheres were prepared by mixing the two solutions together (the total mass of the AIE molecules accounted for 1 wt% of the mass of the blank polymer microspheres), ultrasonically treating them at a power of 100 W for 1 min, sealing and swelling for 2 h, and then evaporating the solvent for 4 h. The supernatant was removed by centrifugation to obtain the AIE polymer microspheres. The obtained AIE polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h. The microspheres were centrifuged at 5000 rpm and resuspended in water. The reaction was repeated three times to obtain the AIE polymer microspheres with sulfonated surfaces.
[0077] Ferrous sulfate heptahydrate and ferric chloride hexahydrate were mixed with 100g water in a mass ratio of 2:1 (the total mass of iron salt accounted for 5wt% of the mass of blank polymer microspheres), and the AIE polymer microspheres with sulfonation modified on the surface obtained above were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 50mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80℃, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
[0078] The morphology of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was observed using a field emission SEM electron microscope. The microspheres showed a regular spherical structure with a statistical particle size of about 5μm. The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R1 was 620nm, and the ratio of the fluorescence intensity before and after the coating of AIE-R1 was 1100. The emission wavelength of AIE-IR2 was 1000nm, and the ratio of the fluorescence intensity before and after the coating of AIE-IR2 was 1500. The difference in central wavelength was 380nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the tested flow fluorescence signal was 24.6%, and the CV value of the flow FCS was 19.7%, indicating encoding failure.
[0079] Comparative Example 3
[0080] Weigh 1 g of blank polymer microspheres and disperse them in 100 g of water to obtain a microsphere dispersion;
[0081] 5 mg of fluorescein-1 molecule (FITC) and 5 mg of fluorescein-2 (CY5) molecule were dissolved in 10 mL of tetrahydrofuran to obtain an AIE swelling agent solution; the two solutions were mixed together (the total mass of fluorescein molecules accounted for 1 wt% of the mass of blank polymer microspheres), and ultrasonically treated at a power of 100 W for 1 min. After the swelling was closed for 2 h, the supernatant was removed by centrifugation and the solvent was volatilized for 4 h to obtain fluorescein polymer microspheres. The obtained fluorescein polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at 5000 rpm and resuspended in water, and the reaction was repeated three times to obtain fluorescein polymer microspheres with sulfonated surface modification.
[0082] Ferrous sulfate heptahydrate and ferric chloride hexahydrate were mixed with 100g water in a mass ratio of 2:1 (the total mass of iron salt accounted for 5wt% of the mass of blank polymer microspheres), and the above-obtained sulfonated surface-modified fluorescein polymer microspheres were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. This process was repeated three times to obtain iron-chelated fluorescein polymer microspheres. 50mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the fluorescein polymer microspheres. The microspheres were centrifuged at 5000rpm and resuspended in water. This process was repeated three times to obtain dual-wavelength fluorescein magnetically encoded microspheres.
[0083] The morphology of the dual-wavelength fluorescein magnetically encoded microspheres was observed using a field emission SEM electron microscope. The microspheres showed a regular spherical structure with a statistical particle size of about 5μm. The fluorescence spectrum of the dual-wavelength fluorescein magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of fluorescein-1 was 520nm, and the ratio of the fluorescence intensity before and after the coating of fluorescein-1 was 1.12. The emission wavelength of fluorescein-2 was 664nm, and the ratio of the fluorescence intensity before and after the coating of fluorescein-2 was 0.95. The difference in central wavelength was 144nm. The encoding data of the dual-wavelength fluorescein magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the tested flow fluorescence signal was 24.6%, and the CV value of the flow FCS was 19.7%, indicating that the encoding failed.
[0084] Comparative Example 4
[0085] Weigh 1 g of blank polymer microspheres and disperse them in 100 g of water to obtain a microsphere dispersion;
[0086] 5 mg of quantum dot-1 (CdSe / ZnS) and 5 mg of quantum dot-2 (CdSe / CdS) were dissolved in 10 mL of tetrahydrofuran to obtain a quantum dot swelling agent solution; the two solutions were mixed together (the total mass of quantum dots accounted for 1 wt% of the mass of blank polymer microspheres), and ultrasonically treated at a power of 100 W for 1 min, and after closed swelling for 2 h, the solvent was evaporated open for 4 h, and the supernatant was removed by centrifugation to obtain quantum dot polymer microspheres. The obtained quantum dot polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and repeated three times to obtain quantum dot polymer microspheres with sulfonated surface modification.
[0087] Ferrous sulfate heptahydrate and ferrous chloride hexahydrate were mixed with 100g water in a mass ratio of 2:1 (the total mass of iron salt accounted for 5wt% of the mass of blank polymer microspheres), and the above-obtained quantum dot polymer microspheres with sulfonation surface were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated quantum dot polymer microspheres; 50mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80℃, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles which were deposited on the surface of the quantum dot polymer microspheres; the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength quantum dot magnetically encoded microspheres.
[0088] The morphology of the dual-wavelength quantum dot magnetically encoded microspheres was observed using a field emission SEM electron microscope. The microspheres showed a regular spherical structure with a statistical particle size of about 5μm. The fluorescence spectrum of the dual-wavelength quantum dot magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of quantum dot-1 was 610nm, and the ratio of the fluorescence intensity of quantum dot-1 before and after coating was 1.13. The emission wavelength of quantum dot-2 was 780nm, and the ratio of the fluorescence intensity of quantum dot-2 before and after coating was 1.11. The difference in central wavelength was 170nm. The encoding data of the dual-wavelength quantum dot magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal tested was 20.6%, and the CV value of the flow FCS was 17.7%, indicating encoding failure.
[0089] The results of the microspheres encoded with different fluorescent materials in Example 1 and Comparative Examples 1-4 are shown in Table 1.
[0090] Table 1 Effects of different wavelengths of AIE fluorescent microspheres, fluorescein microspheres and quantum dot microspheres on flow encoding results
[0091]
[0092] Example 2
[0093] Weigh 0.5 g of blank polymer microspheres and disperse them in 50 g of water to obtain a microsphere dispersion;
[0094] 5 mg of AIE-R1 molecules (alkyl chain-C 8 H 17 The AIE polymer microspheres were prepared by mixing the two solutions together, ultrasonically treating them at a power of 100 W for 1 min, sealing and swelling for 2 h, evaporating the solvent for 4 h, and centrifuging to remove the supernatant. The obtained AIE polymer microspheres were added to 30 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h. The microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and the reaction was repeated three times to obtain AIE polymer microspheres with sulfonated surfaces.
[0095] A total mass of 0.05 g of ferrous sulfate heptahydrate and ferric chloride hexahydrate was mixed with 50 g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1 hour, the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 30 mL of 1 mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0096] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R1 was 620nm, and the ratio of the fluorescence intensity before and after AIE-R1 coating was 1300. The emission wavelength of AIE-IR3 was 790nm, and the ratio of the fluorescence intensity before and after AIE-IR3 coating was 1400. The difference in central wavelength was 170nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 3.6%, the CV value of the flow FCS was 2.7%, the encoding peak was 24-fold, and the encoding was successful.
[0097] Example 3
[0098] Weigh 1 g of blank polymer microspheres and disperse them in 75 g of water to obtain a microsphere dispersion;
[0099] 25 mg of AIE-R3 molecules and 5 mg of AIE-IR4 molecules were dissolved in 7.5 mL of dichloromethane to obtain an AIE swelling agent solution; the two solutions were mixed together, ultrasonically treated at a power of 100 W for 5 min, closed and swollen for 2 h, and then the solvent was evaporated for 4 h, and the supernatant was removed by centrifugation to obtain AIE polymer microspheres. The obtained AIE polymer microspheres were added to 75 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and repeated three times to obtain AIE polymer microspheres with sulfonated surface modification.
[0100] A total mass of 0.5 g of ferrous sulfate heptahydrate and ferric chloride hexahydrate was mixed with 100 g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1 hour, the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 75 mL of 1 mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0101] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R3 was 630nm, the ratio of the fluorescence intensity before and after AIE-R3 coating was 1250, the emission wavelength of AIE-IR4 was 900nm, the ratio of the fluorescence intensity before and after AIE-IR4 coating was 1250, and the difference in central wavelength was 270nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 2.6%, the CV value of the flow FCS was 4.3%, the encoding peak was 24-fold, and the encoding was successful.
[0102] Example 4
[0103] Weigh 2.5 g of blank polymer microspheres and disperse them in 150 g of water to obtain a microsphere dispersion;
[0104] 50 mg of AIE-R6 molecules and 50 mg of AIE-IR1 molecules were dissolved in 15 mL of tetrahydrofuran to obtain an AIE swelling agent solution; the two solutions were mixed together, ultrasonically treated at a power of 100 W for 5 min, closed and swollen for 2 h, and then the solvent was evaporated for 6 h, and the supernatant was removed by centrifugation to obtain AIE polymer microspheres. The obtained AIE polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and repeated three times to obtain AIE polymer microspheres with sulfonated surface modification.
[0105] A total mass of 0.5 g of ferrous chloride heptahydrate and ferric chloride hexahydrate was mixed with 75 g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1 hour, the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 50 mL of 1 mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0106] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R6 was 620nm, and the ratio of the fluorescence intensity before and after the coating of AIE-R6 was 1350. The emission wavelength of AIE-IR1 was 780nm, and the ratio of the fluorescence intensity before and after the coating of AIE-IR1 was 1150. The difference in the central wavelength was 160nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 5.6%, the CV value of the flow FCS was 6.3%, the encoding peak was 24-fold, and the encoding was successful.
[0107] Example 5
[0108] Weigh 10 g of blank polymer microspheres and disperse them in 500 g of water to obtain a microsphere dispersion;
[0109] 150 mg of AIE-R8 molecules and 5 mg of AIE-IR7 molecules were dissolved in 25 mL of dichloromethane to obtain an AIE swelling agent solution; the two solutions were mixed together, ultrasonically treated at a power of 100 W for 10 min, closed and swollen for 2 h, and then the solvent was evaporated for 10 h, and the supernatant was removed by centrifugation to obtain AIE polymer microspheres. The obtained AIE polymer microspheres were added to 100 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and repeated three times to obtain AIE polymer microspheres with sulfonated surface modification.
[0110] A total mass of 1g of ferrous chloride heptahydrate and ferric chloride hexahydrate was mixed with 50g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1h, the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 100mL of 1mol / L sodium hydroxide solution was added, the temperature was raised to 80℃, and the reaction was carried out for 2h. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0111] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R8 was 660nm, the ratio of the fluorescence intensity before and after AIE-R8 coating was 1550, the emission wavelength of AIE-IR7 was 890nm, the ratio of the fluorescence intensity before and after AIE-IR7 coating was 1150, and the difference in central wavelength was 230nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 7.6%, the CV value of the flow FCS was 3.2%, the encoding peak was 24-fold, and the encoding was successful.
[0112] Example 6
[0113] Weigh 0.1 g of blank polymer microspheres and disperse them in 12.5 g of water to obtain a microsphere dispersion;
[0114] 1 mg mass of AIE-R11 molecules (alkyl chain-C 6 H 13 The AIE polymer microspheres were prepared by mixing the two solutions together, ultrasonically treating them at a power of 100 W for 1 min, sealing and swelling for 2 h, evaporating the solvent for 4 h, and centrifuging to remove the supernatant to obtain the AIE polymer microspheres. The obtained AIE polymer microspheres were added to 15 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at 5000 rpm, and then resuspended in water, and the reaction was repeated three times to obtain the AIE polymer microspheres with sulfonated surface.
[0115] A total mass of 0.02 g of ferrous sulfate heptahydrate and ferric chloride hexahydrate was mixed with 20 g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1 hour, the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 15 mL of 1 mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0116] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R11 was 635nm, and the ratio of the fluorescence intensity before and after the coating of AIE-R11 was 1350. The emission wavelength of AIE-IR6 was 795nm, and the ratio of the fluorescence intensity before and after the coating of AIE-IR6 was 1450. The difference in the central wavelength was 160nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 4.6%, the CV value of the flow FCS was 5.2%, the encoding peak was 24-fold, and the encoding was successful.
[0117] Example 7
[0118] Weigh 1 g of blank polymer microspheres and disperse them in 125 g of water to obtain a microsphere dispersion;
[0119] 50 mg of AIE-R15 molecules and 50 mg of AIE-IR8 molecules were dissolved in 5 mL of dichloromethane to obtain an AIE swelling agent solution; the two solutions were mixed together, ultrasonically treated at a power of 100 W for 1 min, closed and swollen for 2 h, and then the solvent was evaporated for 4 h, and the supernatant was removed by centrifugation to obtain AIE polymer microspheres. The obtained AIE polymer microspheres were added to 50 mL of concentrated sulfuric acid (98.3 wt%), the temperature was raised to 80 ° C, and the reaction was carried out for 8 h; the microspheres were centrifuged at a speed of 5000 rpm, and then resuspended in water, and repeated three times to obtain AIE polymer microspheres with sulfonated surface modification.
[0120] A total mass of 0.2 g of ferrous sulfate heptahydrate and ferric chloride hexahydrate was mixed with 100 g of water in a mass ratio of 2:1, and the AIE polymer microspheres with sulfonation modification obtained above were added. After soaking and reacting for 1 hour, the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain iron salt chelated AIE polymer microspheres; 50 mL of 1 mol / L sodium hydroxide solution was added, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. The iron salt reacted in situ to generate magnetic particles that were deposited on the surface of the AIE polymer microspheres; the microspheres were centrifuged at 5000 rpm and resuspended in water. The process was repeated three times to obtain dual-wavelength aggregation-induced emission magnetically encoded microspheres.
[0121] The fluorescence spectrum of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using a fluorescence spectrometer. The emission wavelength of AIE-R15 was 625nm, and the ratio of the fluorescence intensity before and after the coating of AIE-R15 was 1250. The emission wavelength of AIE-IR8 was 785nm, and the ratio of the fluorescence intensity before and after the coating of AIE-IR8 was 1550. The difference in the central wavelength was 160nm. The encoding data of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres was tested using an analytical flow cytometer. The CV value of the flow fluorescence signal was 5.3%, the CV value of the flow FCS was 3.2%, the encoding peak was 24-fold, and the encoding was successful.
[0122] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. A dual-wavelength aggregation-induced luminescence magnetically encoded microsphere, characterized in that: The method comprises AIE polymer microspheres and magnetic particles; the AIE polymer microspheres are obtained by embedding AIE molecules inside blank polymer microspheres, and the magnetic particles are deposited on the surface of the AIE polymer microspheres; the AIE molecules include AIE-R molecules and AIE-IR molecules; The difference between the maximum emission wavelength of the AIE-IR molecule and the maximum emission wavelength of the AIE-R molecule is in the range of 160 nm to 290 nm, and satisfies Δλ≥185. Where I / I0 is the average value of the fluorescence intensity ratio of AIE-R molecules and AIE-IR molecules before and after embedding, λ IR is the maximum emission wavelength of the AIE-IR molecule, λ R is the maximum emission wavelength of the AIE-R molecule.
2. The dual-wavelength aggregation-induced luminescence magnetically encoded microsphere according to claim 1, characterized in that: The blank polymer microspheres are selected from at least one of polystyrene microspheres, polymethyl methacrylate microspheres and polyglycidyl acrylate microspheres; The magnetic particles are Fe3O4; The AIE-R molecule is selected from one of the following AIE-R1 to AIE-R16 molecules: The AIE-IR molecule is selected from one of the following AIE-IR1 to AIE-IR10 molecules:
3. The dual-wavelength aggregation-induced luminescence magnetically encoded microsphere according to claim 1, characterized in that: The AIE molecules are embedded in the blank polymer microspheres by an active swelling method, wherein the amount of the AIE molecules used in the active swelling method is 0.01-10wt% of the amount of the blank polymer microspheres, wherein the mass amount of the AIE-R molecules accounts for 0.01% to 1000% of the mass amount of the AIE-IR molecules; The magnetic particles are deposited on the surface of the AIE polymer microspheres by an in-situ precipitation method of iron salts, wherein the amount of iron salts used in the in-situ precipitation method is 0.1-25 wt % of the amount of blank polymer microspheres used.
4. The dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to claim 3, characterized in that: The active swelling method is to allow the AIE molecules to swell with the blank polymer microspheres through a swelling agent so that the AIE molecules are embedded inside the blank polymer microspheres; The in-situ precipitation method is to add an alkaline solution to react with the iron salt chelated on the surface of the AIE polymer microsphere in situ to generate magnetic particles that are deposited on the surface of the AIE polymer microsphere.
5. The dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to claim 4, characterized in that: In the active swelling method, the swelling agent is selected from at least one of dichloromethane, tetrahydrofuran, chloroform, anisole, benzyl alcohol and toluene, and the particle size of the blank polymer microspheres ranges from 0.03 μm to 50 μm; In the in-situ precipitation method, the surface of the AIE polymer microspheres is modified by sulfonation, the alkaline solution is selected from at least one of sodium hydroxide solution, ammonia water, potassium hydroxide solution and sodium bicarbonate solution; the iron salt is selected from at least one of trivalent iron salt and divalent iron salt; the trivalent iron salt is selected from at least one of ferric chloride hexahydrate and anhydrous ferric chloride; the divalent iron salt is selected from at least one of ferrous chloride tetrahydrate, ferrous chloride dihydrate, ferrous sulfate and ferrous sulfate heptahydrate.
6. The dual-wavelength aggregation-induced luminescence magnetically encoded microsphere according to claim 1, characterized in that: The encoding capacity of the dual-wavelength aggregation-induced luminescence magnetic encoding microspheres is ≥24, and the CV value of the flow fluorescence signal and the CV value of the flow FCS are both less than 10%.
7. The method for preparing dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to any one of claims 1 to 6, characterized in that: The steps include: S1. Preparation of AIE polymer microspheres by active swelling method (1) dispersing blank polymer microspheres in water to obtain a microsphere dispersion; (2) dissolving the AIE molecules in a swelling agent to obtain an AIE swelling agent solution; (3) adding the AIE swelling agent solution of step (2) to the microsphere dispersion of step (1), and after ultrasonic treatment, closing the reactor to carry out swelling reaction. After the reaction is completed, volatilizing and removing the swelling agent to obtain AIE polymer microspheres; S2. Preparation of dual-wavelength aggregation-induced luminescence magnetically encoded microspheres by in situ precipitation The AIE polymer microspheres of step S1 are dissolved in a sulfuric acid solution, the temperature is increased for reaction, and the supernatant is removed by centrifugation to obtain AIE polymer microspheres with sulfonation-modified surfaces. The AIE polymer microspheres are mixed with iron salt and water for reaction, and the supernatant is removed by centrifugation to obtain iron salt-chelated AIE polymer microspheres. An alkaline solution is added, and the temperature is increased. The iron salt reacts in situ to generate magnetic particles that are deposited on the surface of the AIE polymer microspheres. The supernatant is removed by centrifugation to prepare dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
8. The method for preparing dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to claim 7, characterized in that: The following steps are involved: S1. Preparation of AIE polymer microspheres by active swelling method (1) dispersing blank polymer microspheres in water to obtain a microsphere dispersion; (2) dissolving the AIE molecules in a swelling agent to obtain an AIE swelling agent solution; (3) adding the AIE swelling agent solution described in step (2) to the microsphere dispersion described in step (1), and after ultrasonic treatment at an ultrasonic power of 50 W to 400 W for 1 min to 30 min, a closed reactor is used for swelling reaction for 0.5 h to 4 h. After the reaction is completed, the swelling agent is volatilized to obtain AIE polymer microspheres; S2. Preparation of dual-wavelength aggregation-induced luminescence magnetically encoded microspheres by in situ precipitation The AIE polymer microspheres of step S1 are dissolved in a sulfuric acid solution, the temperature is raised to 30°C to 100°C and the reaction is carried out for 4h to 12h, and the supernatant is removed by centrifugation to obtain AIE polymer microspheres with sulfonation modified on the surface. The microspheres are mixed with iron salt and water, and the mixture is immersed in the solution for reaction for 0.5h to 10h, and the supernatant is removed by centrifugation to obtain iron salt chelated AIE polymer microspheres. An alkaline solution is added, and the temperature is raised to 60°C to 120°C and the reaction is carried out for 0.5h to 4h. The iron salt reacts in situ to generate magnetic particles which are deposited on the surface of the AIE polymer microspheres. The supernatant is removed by centrifugation to prepare dual-wavelength aggregation-induced luminescence magnetically encoded microspheres.
9. The method for preparing dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to claim 8, characterized in that: In step S1, the mass amount of blank polymer microspheres in the microsphere dispersion is 0.1% to 20% of the mass amount of water; In step S1, the mass amount of the AIE molecules in the AIE swelling agent solution is 0.1% to 50% of the mass amount of the swelling agent; In step S2, the mass concentration of the sulfuric acid solution is 70% to 99%; the mass amount of the AIE polymer microspheres is 1% to 30% of the mass amount of the sulfuric acid solution; In step S2, the mass dosage of the iron salt is 0.0005% to 25% of the mass dosage of water; the mass dosage of the alkaline solution is 0.1% to 50% of the mass dosage of water; the mass concentration of the alkaline solution is 1% to 10%; The water in step S1 and step S2 is ultrapure water; the centrifugal speed is 3000 rpm to 6000 rpm, the centrifugal time is 5 min to 60 min, and the number of centrifugation is more than three times.
10. Use of the dual-wavelength aggregation-induced luminescence magnetically encoded microspheres according to any one of claims 1 to 6 in in vitro non-disease diagnostic testing.
Citation Information
Patent Citations
Fluorescent encoding microspheres and arrays and preparation method of fluorescent encoding microsphere
CN112111268A
Preparation method of aggregation-induced emission microspheres with core-shell structure
CN114672301A