A synergistic high ionic conductivity carbon film and its preparation method and application
By using multi-walled carbon nanotubes and metal oxide coatings combined with biofiber carbon film technology on the interlayer of lithium metal batteries, the problem of insufficient ion conductivity in the interlayer of lithium metal batteries is solved and the suppression of lithium dendrites is achieved. and high energy density battery performance.
Patent Information
- Application Number
- CN202410131187.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-31
AI Technical Summary
The insufficient ion conductivity of the interlayer in lithium metal batteries leads to the growth of lithium dendrites and low Coulombic efficiency. It is difficult to effectively solve this problem with existing technology.
Using multi-walled carbon nanotubes as the basis, ozone technology is used to construct defects and the ALD atomic layer deposition method is used to coat the metal oxides ZnO and AlPO4. Combined with biological fibers, a carbon film with synergistic high ion conductivity is formed through the carbonization process to enhance lithium ionic conductivity and inhibits lithium dendrite growth.
It significantly improves the lithium ion conductivity, extends the service life of the electrode, achieves high energy density and uniform growth of lithium metal anode, and reduces the manufacturing cost of the battery.
Smart Images

Figure CN118040235B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium metal batteries, and specifically relates to a method for preparing a synergistic high ionic conductivity carbon film. At the same time, it also relates to a synergistic high ionic conductivity carbon film prepared by the preparation method, which is used for the intermediate layer of a lithium metal battery. Background Art
[0002] Lithium-ion batteries (LIBs) are a type of secondary battery system developed in the last century. In 1991, after six years of research and development, Sony's first LIBs product was launched. The structure of this battery is relatively simple, and it has the characteristics of high power density, high energy conversion efficiency, low temperature start-up, no pollution, and light weight. The main components of LIBs are positive electrode, negative electrode, separator, and electrolyte. The negative electrode is an important component of LIBs. Most of the commercial LIBs currently used on the market use graphite as the negative electrode. The function of the negative electrode is to accommodate and collect Li from the positive electrode. + The development of traditional lithium-ion batteries with graphite negative electrodes has approached the upper limit of their theoretical capacity (372mAh / g). Lithium metal batteries have begun to be sought after by scientific researchers around the world due to their high theoretical capacity (3860mAh / g) and low reduction potential (-3.04V, vs standard hydrogen electrode). The high activity of lithium metal makes lithium metal batteries (LMBs) face severe safety issues and low coulombic efficiency caused by dendrite growth during the cycle. Currently, several mainstream solutions include designing functional electrolytes, constructing special three-dimensional current collectors, and modifying artificial solid electrolyte membranes, all of which are aimed at solving the problem of lithium dendrite growth. The earliest application of carbon materials in LIBs batteries can be traced back to the last century, and they are also widely used in LMBs. In LMBs, the use of lithium-philic interlayers is the most critical step in inhibiting dendrite growth and exerting the high capacity of lithium metal batteries. It not only requires the interlayer to have excellent conductivity to achieve rapid conduction of electrons and ions, but also requires strong chemical stability to avoid side reactions with electrolytes. In addition, the unique lithium-philic mechanism of the interlayer is also the key to achieving dendrite-free lithium metal negative electrodes. The lithium-philic interlayer carbon film is closely related to the production cost and battery efficiency of lithium metal batteries. It can be said that the presence or absence of the carbon film directly affects the performance and service life of LMBs.
[0003] LIBs are a kind of high energy density battery. LiCoO2 (LCO) is the first generation of commercial lithium-ion battery cathode material and still occupies the main market of lithium-ion secondary battery cathode material. Its working principle is as follows: when charging, the cathode undergoes oxidation reaction, e - Through the external circuit from the positive to the negative electrode, the Li inside the battery + The electrolyte goes from the positive electrode to the negative electrode, where a reduction reaction occurs. Contrary to the charging process, a reduction reaction occurs at the positive electrode during discharge. -From the negative electrode to the positive electrode through the external circuit, the Li inside the battery + The electrolyte passes from the negative electrode to the positive electrode, and an oxidation reaction occurs at the negative electrode. The electrochemical reactions that occur during the charge and discharge process of a lithium-ion battery using LiCoO2 as the positive electrode material and graphite carbon as the negative electrode are as follows:
[0004] Positive electrode reaction:
[0005] Negative electrode reaction:
[0006] Overall reaction:
[0007] The energy density and lithium storage capacity of the negative electrode in LIBs are the main factors affecting battery performance, and the corresponding component is the lithium metal anode (LMA). Conventional LMA is mainly composed of pure lithium foil. LMA faces safety hazards and low coulombic efficiency (CE) caused by lithium dendrite growth during the cycle. When a carbon film is used as an interlayer, the transfer efficiency of ions and electrons is affected to a certain extent due to the addition of the interlayer when the carbon film is combined with LMA.
[0008] Requirements that the mezzanine needs to meet:
[0009] (1) High ionic and electronic conductivity. Since the interlayer needs to be used as a channel during the propagation of electrons between lithium metal and the interlayer, and the current needs to be collected, the ionic and electronic conductivity of the interlayer are required to be very high.
[0010] (2) High strength. In order to ensure the stability of the electrode, the overall structure of the electrode must be stable, thereby extending the service life of the electrode.
[0011] (3) It has high porosity and pore size distribution in a specific range. + It is the main medium for penetration, nucleation, diffusion and growth, so it must have a high porosity and a certain pore distribution to ensure the uniform growth of lithium metal and avoid the occurrence of lithium dendrites.
[0012] (4) Good corrosion resistance. Because it has to work under oxidation and reduction conditions for a long time, it has high requirements for its corrosion resistance and corrosion resistance.
[0013] (5) It has suitable lithium affinity. + Appropriate adsorption energy helps to adjust Li + nucleation and growth, improving the morphology of lithium metal deposition.
[0014] (6) With dense structure and flat surface. The compact and smooth carbon film can reduce the contact resistance and improve its conductivity. Summary of the invention
[0015] The present invention provides a method for preparing a synergistic high ionic conductivity carbon film to solve the problem of lithium dendrite growth and low coulomb efficiency caused by the obstruction of ionic conductivity caused by the application of the intermediate layer of the current lithium metal battery, thereby solving the problem of high energy density lithium metal battery towards practical application. Different coating circles have an effect on the Li + The increase in conductivity has different effects.
[0016] In order to solve the above problems, the present invention adopts the following technical solutions:
[0017] In a first aspect, the present invention provides a method for preparing a synergistic high ionic conductivity carbon film, comprising the following steps:
[0018] (1) A layer of defects was constructed on the surface of multi-walled carbon nanotubes M-GRADE MWNTs using ozone technology, and then metal oxides ZnO and AlPO4 were coated to 11 to 20 nm using ALD atomic layer deposition, and the multi-walled carbon nanotubes coated with metal oxides ZnO and AlPO4 were mixed in a mass ratio of 2:1 to 1:1;
[0019] (2) After mixing the multi-walled carbon nanotubes and biofibers obtained in step (1), add anhydrous ethanol, stir evenly using a wall-breaking machine, then add a polyacrylamide solution to the slurry for bonding, stir evenly at a slow speed, then filter and dry to obtain a multi-walled carbon nanotube / biofiber membrane, wherein the surface density of the multi-walled carbon nanotube / biofiber membrane is controlled at 1 mg cm -2 ;
[0020] (3) placing the multi-walled carbon nanotube / biofiber membrane obtained in step (2) into a tubular furnace, heating it to 600°C at a heating rate of 2°C per minute under room temperature under an inert gas argon atmosphere, and keeping it warm for 5 hours. After cooling to room temperature, taking it out to obtain the carbon membrane.
[0021] Furthermore, the multi-walled carbon nanotubes in step (2) have a diameter of 70-80 nm and a length of 1-2 mm, and the biofibers in step (2) have a diameter of 7-10 μm and a length of 5 mm.
[0022] Furthermore, the purpose of the carbonization in step (3) is to remove the biofibers, avoid the subsequent dissolution of the biofibers leading to the decomposition of the carbon film, and stabilize the structure of the carbon film.
[0023] As described above, the carbon film used for the middle layer of lithium metal battery prepared by the above method uses the unique lithium conduction mechanism of ZnO and Al2O3 as a means to improve the lithium ion conductivity, uses multi-walled carbon nanotubes as the carbon film layer, and the biofiber further makes the supporting structure of the carbon film more stable. ZnO and AlPO4 are deposited on the multi-walled carbon nanotubes with the same thickness respectively, and the improvement of ion conductivity by individual action and synergistic action is also different.
[0024] In the above scheme of the present invention, the unique ALD technology in step (1) can achieve kilogram-level multi-walled carbon nanotube powder modification, can achieve the market production of high ionic conductivity materials, greatly reduce the cost of lithium metal battery market application, and the synergistic effect of ZnO and AlPO4 plays a significant advantage in improving ionic conductivity. The polyacrylamide in step (2) is a dispersant, which contains amide groups and is easy to form hydrogen bonds, so that the mixed solution has good water solubility and high chemical activity. It also has the ability to reduce the viscosity of the aqueous solution and is easy to disperse the insoluble phase in the mixed solution. The main purpose of adding biofiber in step (2) is to increase the porosity of the carbon film and make the distribution of multi-walled carbon nanotubes more uniform. In the carbonization process in step (3), the heating rate is increased from 2°C per minute to 600°C. As the temperature increases, the functional groups and chemical bonds inside the carbon film and the biofiber are removed by carbonization, increasing the porosity of the carbon film and stabilizing the carbon film structure. If the temperature is too high, the maintenance frequency of the equipment increases, and the cost of consumption is also greatly increased. The carbonization temperature is selected to be 600°C, which controls the cost while ensuring high porosity in the carbon membrane.
[0025] In the scheme of the present invention, the biofiber used is short-cut biofiber with a diameter of 7-10μm and a length of 5mm, in order to increase the porosity of the carbon film. The multi-walled carbon nanotubes used are M-GRADE MWNTs with a diameter of 70-80nm. M-GRADE MWNTs are a kind of long multi-walled carbon nanotubes, which are better in softness than other carbon materials, not easy to break, more conductive, better in film-forming ability, and light in weight, which greatly reduces the manufacturing cost. The unique ALD technology used has the advantage of kilogram-level mass production, which is a significant commercial advantage of this product.
[0026] In the second aspect, the present invention provides a synergistic high ionic conductivity carbon film prepared by the above method, which is based on multi-walled carbon nanotubes and first proposes metal oxides ZnO and AlPO4 as unique Li + The conductivity of the material regulates the significant advantage of uniform lithium metal deposition, and the synergistic effect of ZnO and AlPO4 on Li + The improvement of conductivity has a significant effect, ZnO and Li + The reaction produces Li2O and Li +LiZn alloy with low migration barrier, AlPO4 does not participate in Li + The electrochemical reaction of migration, in the conduction Li + The synergistic effect of the two significantly improves the ionic conductivity of the carbon membrane, and the addition of biofiber gives the carbon membrane a suitable porosity.
[0027] In the third aspect, the present invention provides a synergistic high ionic conductivity carbon film for the intermediate layer of a lithium metal battery, which catalyzes the effective conduction and uniform growth of lithium metal during the lithium nucleation process, inhibits the dendrite growth of the lithium metal negative electrode, and enables the high energy density of the lithium metal negative electrode to be put into practical use.
[0028] Compared with the prior art, the present invention has the following technical effects: From the characteristics of lithium metal batteries, it can be seen that the synergistic effect of ZnO and AlPO4 can improve the performance of Li + The conductivity and the inhibition of the growth of lithium dendrites have significant effects. ZnO and Li + The reaction produces Li2O and Li + LiZn alloy with low migration barrier, AlPO4 does not participate in Li + The electrochemical reaction of migration, in the conduction Li + The synergistic effect of the two significantly improves the ionic conductivity of the carbon membrane, and on this basis, improves the interlayer's resistance to Li + The conductivity can bring out the significant advantage of the high energy density of lithium metal batteries. The negative electrode collects the Li required for electrochemical reduction. + and Li generated by electrochemical reduction 0 The cathode diffusion layer releases Li through electrochemical oxidation reaction + Multi-walled carbon nanotubes are a kind of highly conductive carbon material with excellent comprehensive performance. In addition to high conductivity, they are also corrosion-resistant, wear-resistant, high-temperature-resistant, high-strength, and light-weight. Therefore, they have become the preferred material for making the interlayer of lithium metal batteries. Lithium-phobic materials will aggravate the growth of lithium dendrites, bring safety hazards and low coulomb efficiency. Low conductivity will increase the internal loss of the electrode, leading to the problem of high efficiency and low cost of the battery. Therefore, in order to effectively transmit electrons and ions in the electrochemical reaction, the interlayer must have a unique conductive Li + Characteristics and excellent electrical conductivity. ZnO and AlPO4 have unique Li + Characteristics, Li + The LiZn alloy generated after nucleation has a low migration barrier and Li2O with high ionic conductivity. AlPO4 is good at conducting Li +It has significant advantages in various aspects, and as a stable structure it does not participate in electrochemical reactions. With the support of multi-walled carbon nanotubes with excellent electrical conductivity, the product of the invention catalyzes the effective conduction and uniform growth of lithium metal during the lithium nucleation process, inhibits the dendrite growth of the lithium metal negative electrode, and makes the high energy density of the lithium metal negative electrode practical. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a physical picture of the carbon film in step (2) of Example 1 of the present invention, wherein the size of the carbon film is 13×13 cm.
[0030] Figure 2 The scanning electron microscope images of the carbon film of the present invention are shown in Figure 1, wherein (a) is a 3000-fold magnification of the carbon film in step (3) of Example 1, (b) is a 3000-fold magnification of the carbon film in step (3) of Example 2, and (c) is a 3000-fold magnification of the carbon film in step (3) of Example 3.
[0031] Figure 3 The carbon film prepared in step (3) of Example 1 and step (3) of Example 4 of the present invention is used as the intermediate interlayer of the lithium metal negative electrode and Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2 assembled full cell electrochemical impedance spectroscopy (EIS) test. Example 1 Step (3) Carbon film EIS test results are as follows Figure 3 As shown in blue, the EIS test results of the carbon film in step (3) of Example 4 are as follows Figure 3 The red color indicates that, through the EIS impedance test, it can be found that the ionic conductivity of the carbon film in step (3) of Example 1 is significantly improved after the introduction of ZnO compared with the carbon film in step (3) of Example 4. The performance in the EIS test is that it has a lower interface resistance of 17Ω. Figure 3 As shown in medium blue, the carbon film in step (3) of Example 4 has a large interface resistance and low ionic conductivity.
[0032] Figure 4 The carbon film prepared in step (3) of Example 2 and step (3) of Example 3 of the present invention is used as the intermediate interlayer of the lithium metal negative electrode and Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2 assembled full cell electrochemical impedance spectroscopy (EIS) test. Example 2 Step (3) Carbon film EIS test results are as follows Figure 4 As shown in red, the EIS test results of the carbon film in step (3) of Example 3 are as follows Figure 4The blue color indicates that, through the EIS impedance test, it can be found that the ionic conductivity of the carbon film in step (3) of Example 3 is significantly improved after the introduction of ZnO on the basis of the introduction of AlPO4, compared with the carbon film in step (3) of Example 2. The performance in the EIS test is that it has the lowest interface resistance of 10Ω and high ionic conductivity. Figure 4 As shown in the middle blue, the carbon film in step (3) of Example 4 has a large interface resistance of 50Ω and low ionic conductivity. Figure 4 As shown in red, it is confirmed that the synergistic effect of AlPO4 and ZnO has an irreplaceable effect in high ionic conductivity. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0034] The biofiber used in the following examples is a short-cut biofiber with a diameter of 7-10 μm and a length of 5 mm, which is a carbon fiber; the multi-walled carbon nanotubes used are M-GRADE MWNTs (purchased from nano tech labs) with a diameter of 70-80 nm and a length of 1-2 mm.
[0035] Example 1: A synergistic carbon film for the intermediate layer of a lithium metal battery is prepared by the following method:
[0036] (1) Ozone is used to construct a large number of defects on the surface of multi-walled carbon nanotubes as attachment sites for subsequent deposition of metal oxides, and the unique ALD technology is used to coat the surface of multi-walled carbon nanotubes with different thicknesses of metal oxide ZnO.
[0037] In the above steps, 0.9 mg of multi-walled carbon nanotubes are required for each square centimeter of filter cloth, so that the surface density of the carbon film on the filter cloth reaches 1 mg cm -2 .
[0038] (2) Use anhydrous ethanol as a solvent, mix multi-walled carbon nanotubes and biofibers in a mass ratio of 9:1, mix and stir in a crusher for 3 times, each time for 2 minutes. During this period, rinse the multi-walled carbon nanotubes on the tube wall with anhydrous ethanol to ensure that all multi-walled carbon nanotubes are evenly dispersed. After stirring evenly, pour into a beaker, add 0.05% polyacrylamide aqueous solution with a mass fraction of 1% of the total solution at a speed of 100-300r, reduce the dispersion resistance of the solution, and make the solution evenly dispersed. Filter with a vacuum filtration device, filter the solution on a 500-mesh filter cloth, put the filtered filter cloth into an 80°C blast drying oven, and peel off the multi-walled carbon nanotube / biofiber membrane from the filter cloth after complete drying, which is the desired carbon membrane, such as Figure 1 shown.
[0039] The filter cloth in the above steps has a mesh size of 500. The carbon film peeled off from the filter cloth has a size of 13 cm x 13 cm and a surface density of 1 mg cm. -2 The carbon film can be rolled on a roller press. The distance between the rollers of the roller press is controllable, so the thickness of the carbon film can be controlled to reach 20 to 60 μm. If it is too thick, the porosity and power density will be affected. If it is too thin, the mechanical strength will be insufficient.
[0040] (3) Then, the multi-walled carbon nanotube / biofiber membrane prepared in step (2) was carbonized using a tubular furnace under pure argon flow conditions. The carbonization temperature was 600° C., the heating rate was 2° C. per minute at room temperature, and the temperature was kept at 600° C. for 5 hours. After cooling to room temperature, the carbon membrane was taken out and stored in a vacuum drying oven at 60° C.
[0041] Example 2: A synergistic carbon film is used as an intermediate layer of a lithium metal battery, and is prepared by the following method:
[0042] (1) Ozone is used to construct a large number of defects on the surface of multi-walled carbon nanotubes as attachment sites for subsequent deposition of metal oxides, and AlPO4 coating of different thicknesses is performed on the surface of multi-walled carbon nanotubes using a unique ALD technology.
[0043] The AlPO4 coating with different thicknesses on the surface of multi-walled carbon nanotubes includes the following steps:
[0044] The porous container was placed in the ALD reaction chamber, and vacuum was evacuated and replaced with nitrogen three times. The temperature of the reaction chamber was raised to 200°C, and the pressure of the reaction chamber was maintained at 5 torr.
[0045] Rotating the porous container to allow the multi-walled carbon nanotubes to be fully mixed in the porous cavity;
[0046] The precursor trimethylaluminum vapor is pulsed into the reaction chamber under the N2 flow rate of 50sccm, adsorbed on the multi-walled carbon nanotubes until 6torr, and maintained for 60 seconds, and then 50sccm N2 is used to purge and take away the remaining trimethylaluminum, and the N2 purge time is 30s. Similarly, dimethyl phosphate is pulsed into the reaction chamber under the N2 flow rate of 50sccm until the gas pressure reaches 6torr and maintained for 60 seconds, and reacts with trimethylaluminum that has been chemically adsorbed on the multi-walled carbon nanotubes to generate AlPO4, and the time is 60s. Subsequently, the excess dimethyl phosphate and by-products are taken out of the reaction chamber by 50sccm N2 purge, and the purge time is 30s, thus completing an ALD deposition cycle; repeat this step to coat the multi-walled carbon nanotube surface with AlPO4 of different thicknesses.
[0047] In the above steps, 0.9 mg of multi-walled carbon nanotubes are required for each square centimeter of filter cloth, so that the surface density of the carbon film on the filter cloth reaches 1 mg cm -2 .
[0048] (2) Using anhydrous ethanol as a solvent, multi-walled carbon nanotubes and biofibers are mixed in a mass ratio of 9:1, and mixed and stirred in a crusher for 3 times for 2 minutes each time. During this period, the multi-walled carbon nanotubes on the tube wall are rinsed with anhydrous ethanol to ensure that all multi-walled carbon nanotubes are evenly dispersed. After stirring evenly, pour into a beaker, add 1% of the total solution mass fraction of 0.05% polyacrylamide aqueous solution at a speed of 100-300r to reduce the dispersion resistance of the solution and make the solution evenly dispersed. Filter with a vacuum filtration device, filter the solution on a 500-mesh filter cloth, put the filter cloth after filtration into an 80°C blast drying oven, and peel off the multi-walled carbon nanotube / biofiber membrane from the filter cloth after complete drying, which is the desired carbon membrane.
[0049] The filter cloth in the above steps has a mesh size of 500. The carbon film peeled off from the filter cloth has a size of 13 cm x 13 cm and a surface density of 1 mg cm. -2 The thickness is about 20 to 60 μm. The carbon film can be rolled on a roller press. The distance between the rollers of the roller press is controllable, so the thickness of the carbon film can be controlled to reach 20 to 60 μm. If it is too thick, the porosity and power density will be affected, and if it is too thin, the mechanical strength will be insufficient.
[0050] (3) Then, the multi-walled carbon nanotube / biofiber membrane prepared in step (2) was carbonized using a tubular furnace under pure argon flow conditions. The carbonization temperature was 600° C., the heating rate was 2° C. per minute at room temperature, and the temperature was kept at 600° C. for 5 hours. After cooling to room temperature, the carbon membrane was taken out and stored in a vacuum drying oven at 60° C.
[0051] Example 3: A synergistic carbon film is used as an intermediate layer of a lithium metal battery, and is prepared by the following method:
[0052] (1) Ozone is used to construct a large number of defects on the surface of multi-walled carbon nanotubes as attachment sites for subsequent deposition of metal oxides, and the unique ALD technology is used to coat the multi-walled carbon nanotubes with different thicknesses of ZnO and AlPO4.
[0053] In the above steps, 0.9 mg of multi-walled carbon nanotubes are required for each square centimeter of filter cloth, wherein the mass ratio of multi-walled carbon nanotubes coated with ZnO and multi-walled carbon nanotubes coated with AlPO4 is 1:1, so that the surface density of the carbon film on the filter cloth reaches 1 mg cm -2 .
[0054] (2) Using anhydrous ethanol as a solvent, multi-walled carbon nanotubes and biofibers are mixed in a mass ratio of 9:1, and mixed and stirred in a crusher for 3 times for 2 minutes each time. During this period, the multi-walled carbon nanotubes on the tube wall are rinsed with anhydrous ethanol to ensure that all multi-walled carbon nanotubes are evenly dispersed. After stirring evenly, pour into a beaker, add 1% of the total solution mass fraction of 0.05% polyacrylamide aqueous solution at a speed of 100-300r to reduce the dispersion resistance of the solution and make the solution evenly dispersed. Filter with a vacuum filtration device, filter the solution on a 500-mesh filter cloth, put the filter cloth after filtration into an 80°C blast drying oven, and peel off the multi-walled carbon nanotube / biofiber membrane from the filter cloth after complete drying, which is the desired carbon membrane.
[0055] The filter cloth in the above steps has a mesh size of 500. The carbon film peeled off from the filter cloth has a size of 13 cm x 13 cm and a surface density of 1 mg cm. -2 The thickness is about 20 to 60 μm. The carbon film can be rolled on a roller press. The distance between the rollers of the roller press is controllable, so the thickness of the carbon film can be controlled to reach 20 to 60 μm. If it is too thick, the porosity and power density will be affected, and if it is too thin, the mechanical strength will be insufficient.
[0056] (3) Then, the multi-walled carbon nanotube / biofiber membrane prepared in step (2) was carbonized using a tubular furnace under pure argon flow conditions. The carbonization temperature was 600° C., the heating rate was 2° C. per minute at room temperature, and the temperature was kept at 600° C. for 5 hours. After cooling to room temperature, the carbon membrane was taken out and stored in a vacuum drying oven at 60° C.
[0057] Example 4: A synergistic carbon film is used as an intermediate layer of a lithium metal battery and is prepared by the following method:
[0058] (1) Ozone is used to construct a large number of defects on the surface of multi-walled carbon nanotubes as attachment sites for subsequent deposition of metal oxides, and the unique ALD technology is used to coat the multi-walled carbon nanotubes with different thicknesses of ZnO and AlPO4.
[0059] In the above steps, 0.9 mg of multi-walled carbon nanotubes are required for each square centimeter of filter cloth, wherein the mass ratios of multi-walled carbon nanotubes coated with ZnO and multi-walled carbon nanotubes coated with AlPO4 are 1:1, 2:1, and 1:2, so that the surface density of the carbon film on the filter cloth reaches 1 mg cm -2 .
[0060] (2) Using anhydrous ethanol as solvent, multi-walled carbon nanotubes and biofibers are mixed in a mass ratio of 9:1, and mixed and stirred in a crusher for 3 times for 2 minutes each time. During this period, the carbon nanotubes on the tube wall are rinsed with anhydrous ethanol to ensure that all carbon nanotubes are evenly dispersed. After stirring evenly, pour into a beaker, add 1% of the total solution mass fraction of 0.05% polyacrylamide aqueous solution at a speed of 100-300r to reduce the dispersion resistance of the solution and make the solution evenly dispersed. Filter with a vacuum filtration device, filter the solution on a 500-mesh filter cloth, put the filter cloth after filtration into an 80°C blast drying oven, and peel off the carbon nanotube / biofiber membrane from the filter cloth after complete drying, which is the desired carbon membrane.
[0061] The filter cloth in the above steps has a mesh size of 500. The carbon film peeled off from the filter cloth has a size of 13 cm x 13 cm and a surface density of 1 mg cm. -2 The thickness is about 20 to 60 μm. The carbon film can be rolled on a roller press. The distance between the rollers of the roller press is controllable, so the thickness of the carbon film can be controlled to reach 20 to 60 μm. If it is too thick, the porosity and power density will be affected, and if it is too thin, the mechanical strength will be insufficient.
[0062] (3) Then, the multi-walled carbon nanotube / biofiber membrane prepared in step (1) was carbonized using a tubular furnace under pure argon flow conditions. The carbonization temperature was 600°C, the heating rate was 2°C per minute at room temperature, and the temperature was kept at 600°C for 5 hours. After cooling to room temperature, the carbon membrane was taken out and stored in a vacuum drying oven at 60°C.
[0063] In the above steps, the multi-walled carbon nanotubes and the biofibers are uniformly dispersed in anhydrous ethanol and then filtered through a 500-mesh filter cloth to obtain a carbon film. The multi-walled carbon nanotubes have good conductivity, and the biofibers have a unique supporting effect. The carbon film can be rolled on a roller press. The distance between the rollers of the roller press is controllable, so the thickness of the carbon film can be easily controlled to reach 20 μm. At the same time, the surface density of the carbon film is controlled at 1 mg cm -2, because the size of the carbon film surface density is related to thickness, lithium affinity strength, porosity, density, and tensile strength, among which the relationship is: (1) Thickness: the greater the surface density, the greater the thickness. (2) Lithium affinity strength: The lithium affinity strength of the carbon film is closely related to the morphology of the ALD technology deposit and the surface density of the carbon film. The greater the surface density of the carbon film, the more lithium nucleation sites there are and the stronger the lithium affinity strength. (3) Porosity: It decreases with the increase of the proportion of multi-walled carbon nanotubes. Porosity affects the power density. (4) Density: It increases with the increase of multi-walled carbon nanotubes. (5) Tensile strength: It increases with the increase of carbon paper surface density. A larger surface density is easier to achieve, so at 1 mg·cm -2 It is difficult to ensure uniformity if the surface density is further increased on the basis of , and a large thickness difference will appear in the subsequent carbonization process at 600°C. The method for controlling the surface density in this embodiment is: when the area of the carbon film to be manufactured (the area of the mold used) is known, the mass of the multi-walled carbon nanotubes and the biofiber is weighed, and then the sum of the masses of the two is divided by the area to obtain the surface density.
[0064] In the above steps, 0.9 mg of multi-walled carbon nanotubes and 0.1 mg of biofiber are required for each square centimeter of filter cloth. The aqueous solution containing 0.2% biofiber is used here. The purpose of accurate weighing is to make the carbon paper surface density on the filter cloth reach 1 mg cm -2 After the multi-walled carbon nanotube / carbon fiber membrane is peeled off from the filter cloth, it is rolled on a roller press. The distance between the rollers during rolling is controllable, so the thickness is controllable. The thickness of the multi-walled carbon nanotube / carbon fiber membrane can reach 20 to 60 μm. If it is too thick, its air permeability and power density will be affected, and if it is too thin, its mechanical strength will be insufficient.
[0065] Example 5
[0066] This example tests the ionic conductivity of a steel-to-steel battery based on a modified carbon membrane.
[0067] The assembly method of the steel-on-steel battery is to use steel sheets as both the positive and negative electrodes of the battery, use different carbon films for assembly, and use a Swiss Metrohm electrochemical workstation for corresponding testing. The test results are shown in Table 2.
[0068] Table 1 Ionic conductivity of carbon paper with different ZnO coating thicknesses
[0069] Parameter / Unit Coating thickness / (nm) <![CDATA[Ionic conductivity (S cm -1 )]]> Carbon paper thickness (μm) Example 1 ZnO / 1.5 5.1-5.8 20 Example 1 ZnO / 2.0 5.5-6.3 20 Example 1 ZnO / 7.5 6.1-7.0 20 Example 1 ZnO / 10.5 6.5-7.1 20 Example 1 ZnO / 15.0 5.5-6.8 20
[0070] ZnO has unique Li-conducting + Characteristics, Li + The LiZn alloy generated after nucleation has a low migration barrier and Li2O with high ion conductivity. However, the ZnO coating thickness is not as thick as possible. When the coating thickness is 2.0-7.5nm, the ion conductivity of carbon paper is the highest. If the coating layer is too thick, a large amount of Li+ It will nucleate with ZnO on the surface of the carbon film, causing subsequent lithium metal aggregation deposition to produce dead lithium and lead to Li + The conductivity decreases.
[0071] Table 2 Ionic conductivity of carbon paper with different AlPO4 coating thicknesses
[0072] Parameter / Unit Coating thickness / (nm) <![CDATA[Ionic conductivity (S cm -1 )]]> Carbon paper thickness (μm) Example 2 <![CDATA[AlPO4 / 2.0]]> 2.4-3.1 20 Example 2 <![CDATA[AlPO4 / 4.0]]> 2.5-3.0 20 Example 2 <![CDATA[AlPO4 / 10.0]]> 3.0-3.4 20 Example 2 <![CDATA[AlPO4 / 14.0]]> 2.7-3.0 20 Example 2 <![CDATA[AlPO4 / 20.0]]> 2.2-3.1 20
[0073] AlPO4 has unique Li conductivity + The AlPO4 coating thickness is not as thick as possible. When the coating thickness is 4.0-10.0 nm, the ionic conductivity of carbon paper is the highest. The increase in the thickness of the AlPO4 coating layer does not further improve the ionic conductivity. This may be because as the thickness of the AlPO4 coating layer increases, the Li + During the transport process, random nucleation occurs and uniform deposition is affected, which leads to a decrease in ionic conductivity.
[0074] Table 3 Ionic conductivity of carbon paper under the synergistic effect of ZnO and AlPO4
[0075] Parameter / Unit Coating thickness / (nm) <![CDATA[Ionic conductivity (S cm -1 )]]> Carbon paper thickness (μm) Example 3 <![CDATA[ZnO / 15+AlPO4 / 5]]> 6.5-7.2 20 Example 3 <![CDATA[ZnO / 5+AlPO4 / 15]]> 5.6-6.4 20 Example 3 <![CDATA[ZnO / 15+AlPO4 / 15]]> 8.1-9.3 20 Example 3 <![CDATA[ZnO / 5+AlPO4 / 5]]> 5.1-6.0 20
[0076] When multi-walled carbon nanotubes coated with AlPO4 and ZnO of different thicknesses are mixed in a 1:1 ratio to form a carbon film, the carbon film does not achieve the optimal ionic conductivity only when the multi-walled carbon nanotubes coated with AlPO4 and ZnO each reach the optimal coating thickness. Instead, the carbon film achieves the optimal ionic conductivity through a synergistic effect when the thickness of the AlPO4 and ZnO coated by the multi-walled carbon nanotubes is at a suboptimal value.
[0077] Table 4 Effects of different ratios of multi-walled carbon nanotubes coated with ZnO and multi-walled carbon nanotubes coated with AlPO4 on the ionic conductivity of carbon paper
[0078]
[0079]
[0080] When multi-walled carbon nanotubes coated with 15nm thick AlPO4 and ZnO are mixed in a 1:1 ratio to form a carbon film, the ionic conductivity of the carbon film is the highest. The results show that the synergistic effect of AlPO4 and ZnO on ionic conductivity can exert the best performance when the two have a suitable ratio. At this time, the mechanism of AlPO4 and ZnO in improving ionic conductivity can be fully exerted.
[0081] Table 5 Ionic conductivity of carbon paper of different thicknesses
[0082] Parameter / Unit Coating thickness / (nm) <![CDATA[Ionic conductivity (S cm -1 )]]> Carbon paper thickness (μm) Example 4 0 0.82-1.1 20 Example 4 0 0.70-0.78 30 Example 4 0 0.60-0.70 40 Example 4 0 0.50-0.61 50 Example 4 0 0.46-0.54 60
[0083] It can be seen from Table 5 that carbon paper has higher ionic conductivity at a lower thickness, but due to the lithium-phobicity of the carbon material itself, the Li-conductivity of the carbon material is greatly limited. + Characteristics, leading to Li + Random nucleation on the surface of the carbon film causes the growth of lithium dendrites and the generation of dead lithium, which greatly reduces the ionic conductivity. The thinner the carbon film, the higher the Li + The greater the probability of nucleation through the carbon membrane, this is reflected in the ionic conductivity, a property that is far from meeting the practical requirements of lithium metal batteries.
[0084] Through the above improvements, this embodiment prepares a carbon film with excellent lithium affinity and lower manufacturing cost for the middle layer of lithium metal batteries, and has a sufficiently stable structure to withstand high temperatures and corrosion.
Claims
1. A method for preparing a synergistic high ionic conductivity carbon film, characterized in that: The following steps are involved: (1) A layer of defects was constructed on the surface of multi-walled carbon nanotubes (M-GRADE MWNTs) using ozone technology, and then metal oxides ZnO and AlPO4 were coated to 11-20 nm using ALD atomic layer deposition, and the multi-walled carbon nanotubes coated with metal oxides ZnO and AlPO4 were mixed in a mass ratio of 2:1-1:1; (2) After mixing the multi-walled carbon nanotubes and biofibers obtained in step (1), add anhydrous ethanol and stir evenly using a wall breaker. Then add polyacrylamide solution to the slurry for bonding, stir evenly at a slow speed, and then filter and dry to obtain a multi-walled carbon nanotube / biofiber membrane. The surface density of the multi-walled carbon nanotube / biofiber membrane is controlled at 1 mg cm -2 , the biological fiber is carbon fiber, and the biological fiber is short-cut biological fiber with a diameter of 7-10 μm and a length of 5 mm; (3) The multi-walled carbon nanotube / biofiber membrane obtained in step (2) is placed in a tubular furnace, heated to 600° C. at a heating rate of 2° C. per minute in an inert gas argon atmosphere for carbonization and kept at this temperature for 5 hours. After cooling to room temperature, the membrane is taken out to obtain the carbon membrane.
2. The method for preparing a synergistic high ionic conductivity carbon film according to claim 1, characterized in that: The multi-walled carbon nanotubes in step (2) have a diameter of 70-80 nm and a length of 1-2 mm.
3. The method for preparing a synergistic high ionic conductivity carbon film according to claim 1, characterized in that: The mass ratio of the multi-walled carbon nanotubes to the biofibers in step (2) is 9:
1.
4. The method for preparing a synergistic high ionic conductivity carbon film according to claim 1, characterized in that: In step (2), the amount of anhydrous ethanol added is 200-500 ml, and the amount of polyacrylamide solution added is 3-5 ml.
5. The method for preparing a synergistic high ionic conductivity carbon film according to claim 1 or 4, characterized in that: The polyacrylamide in step (2) is a polyacrylamide aqueous solution with a mass fraction of 0.05%.
6. A synergistic high ionic conductivity carbon film prepared by the preparation method according to any one of claims 1 to 5.
7. A synergistic high ionic conductivity carbon film according to claim 6 used in the middle layer of a lithium metal battery.
8. The use according to claim 7, characterized in that: It uses ZnO and AlPO4 as unique Li + Conductive material, with a multi-walled carbon nanotube / biofiber film composed of multi-walled carbon nanotubes and short-cut biofibers as the carbon film layer, the carbon film layer thickness is 20~60μm, and the surface density is 1mg·cm -2 .
Citation Information
Patent Citations
Lithium metal composite electrode, preparation method thereof and lithium ion battery
CN109546141A
KR20210050059A