Material with dual imaging functions of fluorescence and magnetic resonance imaging and preparation method thereof

The Gd2O(CO3)2·H2O material is prepared by a hydrothermal method doped with high concentration Tb3+, which solves the problems of weak fluorescence emission capability and complex material preparation in the existing technology, and achieves efficient fluorescence and magnetic resonance dual imaging functions, improving improved biosafety and imaging resolution.

CN118048152BActive Publication Date: 2024-10-18HUAIBEI NORMAL UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410056213.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2024-10-18
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

The existing Gd2O(CO3)2·H2O magnetic resonance contrast agent has weak fluorescence emission capabilities, making it difficult to combine fluorescence and magnetic resonance imaging functions. Moreover, the content of Gd element is required under high magnetic fields, resulting in complex material preparation and biological problems. Less secure.

Method used

The high-concentration Tb3+-doped Gd2O(CO3)2·H2O material is prepared by a hydrothermal method. Na2CO3 is used as a reactant to adjust the Tb3+/Gd3+ ion concentration ratio to achieve high fluorescence emission intensity and magnetic resonance imaging functions of the material.

Benefits of technology

The preparation of high-concentration Tb3+ doped materials is achieved, which enhances the fluorescence emission intensity, avoids fluorescence quenching, simplifies the material preparation process, and improves biological safety and imaging functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118048152B_ABST
    Figure CN118048152B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of bioimaging technology, and specifically relates to a material with dual imaging functions of fluorescence and magnetic resonance imaging and a preparation method thereof. The chemical general formula of the material is Gd 2(1‑x) O(CO3)2·H2O:2xTb 3+ , where x is the ratio of Tb 3+ and (Tb 3+ +Gd 3+ ), and 0 < x < 0.8. The use of this material can directly replace the fluorescent dyes required for biofluorescence imaging. At the same time, Gd 3+ in GOC has certain paramagnetism and can be used as a contrast agent for magnetic resonance, enabling the material to have dual imaging functions of fluorescence and magnetic resonance imaging. In addition, the present invention prepares GOC doped with high-concentration Tb 3+ by a hydrothermal method. The ratio of Tb 3+ / Gd 3+ ion concentrations in GOC can be adjusted within a wide range, enabling the material to balance the fluorescence and magnetic resonance imaging quality as needed and improving the resolution of local diseased tissues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of biological imaging technology and relates to a high-concentration Tb 3+ Doped Gd2O(CO3)2 . H2O (denoted as GOC:Tb 3+ ) materials and preparation methods thereof. Background Art

[0002] Gd2O(CO3)2·H2O (denoted as GOC) is a widely used contrast agent for magnetic resonance imaging. 3+ It has a certain paramagnetism, which can change the relaxation time T1 of water molecules in the local soft tissue of the organism, thereby expanding the signal difference between the area and other tissues and enhancing the contrast of magnetic resonance imaging. 3+ of 6 P 7 / 2 to 8 S 7 / 2 Although the energy level transition can emit 311nm ultraviolet light, the fluorescence emission ability is weak, which is not conducive to human eye observation and biological fluorescence imaging. In order to meet the needs of biological imaging, it is often necessary to perform additional dyeing treatments on biological tissues in the preparation stage or to add fluorescent groups to the product to form organic-inorganic composite materials, so that the GOC contrast agent has both fluorescence imaging function.

[0003] In the prior art, the main technical routes for preparing materials with dual functions of fluorescence and magnetic resonance imaging are:

[0004] (1) Urea is selected as the key reactant to generate a GOC magnetic resonance contrast agent, and the fluorescent substance and the Gd-based material are coated into a whole by physical adsorption, embedding or encapsulation to form a magnetic resonance and fluorescence composite material.

[0005] (2) Preparation of Gd-based organic-inorganic composite materials containing fluorescent groups. This type of method requires the prepared Gd-based raw materials, fluorescein and intermediates to be connected to the organic skeleton through a series of chemical reactions to form a whole, thereby generating a composite material with fluorescent groups and Gd-based magnetic resonance imaging function.

[0006] It can be seen that to achieve the dual functions of fluorescence and magnetic resonance imaging, the material must simultaneously meet two conditions: "containing Gd element" and "having fluorescence emission ability". Among them, the Gd element is used for magnetic resonance contrast imaging, and the fluorescence emission ability is used for fluorescence imaging. The magnetic fields of existing mainstream nuclear magnetic resonance equipment are all ultra-high magnetic field intensities of 3T and above, and the requirement for the content of Gd element is not high. Therefore, if the GOC contrast agent can simultaneously emit high-intensity fluorescence, the material preparation process can be greatly simplified, the use of organic chemical reagents can be reduced, and the biosafety of the imaging functional material can be improved.

[0007] Mayama et al. [Y. Mayama et al. Enhancement of the luminescent intensity of the green emitting Gd2O2CO3:Tb phosphor, Journal of Alloys and Compounds, 451 (2008) 132–135] prepared GOC:Tb by solid-state reaction method under the conditions of 600–700 °C and in CO2 atmosphere. 3+ phosphor, and confirmed that Tb 3+ doped GOC has fluorescence emission characteristics, but for the phosphor prepared by this method, fluorescence quenching occurs when the content of Tb 3+ is greater than 17%, and the content of Tb 3+ in the material is not high, and the luminescence intensity needs to be further improved. Summary of the Invention

[0008] To solve the technical problem of limited doping amount of Tb in Gd2O2CO3, the present invention provides a Gd2O(CO3)2 3+ ·H2O material with high-concentration Tb doping and having dual imaging functions of fluorescence and magnetic resonance contrast, and its preparation method. 3+ . H2O material and its preparation method.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A material with dual imaging functions of fluorescence and magnetic resonance contrast, the chemical general formula of the material is Gd 2(1-x) O(CO3)2·H2O:2xTb 3+ , where x is the ratio of Tb 3+ to (Tb 3+ +Gd 3+ ), and 0 < x < 0.8. The use of this material can directly replace the fluorescent dye required for biological fluorescence imaging. At the same time, Gd in GOC 3+ ​It has a certain paramagnetic property and can be used as a contrast agent for magnetic resonance imaging, which enables the material to have dual imaging functions of fluorescence and magnetic resonance imaging. 3+ / Gd 3+ The ratio of ion concentrations can be adjusted over a wide range, allowing the material to take into account both fluorescence and magnetic resonance imaging quality as needed, thereby improving the resolution of local diseased tissue.

[0011] The preparation method of the material is as follows:

[0012] Step 1: absorb Gd(NO3)3 aqueous solution and Tb(NO3)3 aqueous solution in a certain proportion to obtain 2g of nitrate mixed solution with a total amount of metal ions of 1mmol;

[0013] Step 2: Take 20 g of a 5 mol Na2CO3 aqueous solution and place it in a beaker containing a stirrer for later use;

[0014] Step 3: Under the condition that the temperature of the Na2CO3 solution is 15-30°C, the nitrate mixed solution obtained in step 1 is uniformly dropped into the stirred Na2CO3 aqueous solution at a rate of 5 seconds per drop using a rubber-tipped dropper, and vigorously stirred at a speed of 1600-2100 rpm for 5 minutes to obtain a preliminarily mixed nitrate solution;

[0015] Step 4: Add dilute HNO3 dropwise to adjust the pH value of the preliminarily mixed nitrate solution to 8-11;

[0016] Step 5: Monitor the pH value of the solution in real time and keep the pH value of the solution unchanged, and continue to stir vigorously at a speed of 1600-2100 rpm for 30 minutes;

[0017] Step 6: Transfer the stirred solution to a 50 mL reactor, heat to 170-220°C, and keep warm for 360-720 minutes. After the reaction is completed, take out the precipitate in the reactor, wash it with high-purity water three times, and dry it at 40-70°C for 60-200 minutes to obtain the target product.

[0018] In the present invention, high concentration Tb is prepared by hydrothermal method. 3+ Doped GOC, this method is different from the conventional urea method and CO2 atmosphere method. It uses Na2CO3 as a special reactant to prepare high-concentration Tb 3+ Doped GOC has the following advantages over the prior art:

[0019] 1. GOC:Tb prepared by this method 3+ MediumTb 3+ The content is much greater than 17%;

[0020] 2. GOC:Tb 3+The fluorescence emission intensity increases with the 3+ The concentration of α increases with the increase of α, and there is no concentration quenching phenomenon;

[0021] 3. GOC:Tb 3+ Containing Gd and high concentration of Tb, it can be used for both magnetic resonance imaging and high-intensity fluorescence imaging;

[0022] 4. The preparation process is simple, no other additional reactants are involved, the types of reactants are few, the particle size is controllable, the repeatability is good, and it is easy to standardize production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 For GOC: 1Tb 3+ XRD pattern of .

[0024] Figure 2 For GOC: 1Tb 3+ The excitation spectrum.

[0025] Figure 3 For GOC: 1Tb 3+ GOC: 1.4Tb 3+ The emission spectrum of . DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0027] The general chemical formula of the target product obtained in the following examples is Gd 2(1-x) O(CO3)2·H2O:2xTb 3+ , where x is Tb 3+ and (Tb 3+ +Gd 3+ ), 0 <x<0.8。

[0028] Example 1

[0029] Step 1: Take 1 g of each of a 0.5 mmol Gd(NO3)3·6H2O solution and a 0.5 mmol Tb(NO3)3·6H2O solution, mix the two, and obtain 2 g of a rare earth nitrate mixed solution;

[0030] Step 2: Take 20 g of Na2CO3 aqueous solution with a Na2CO3 content of 5 mmol and place it in a beaker containing a stirring bar for later use;

[0031] Step 3: Heat the Na2CO3 aqueous solution to 25°C, and drip the rare earth nitrate mixed solution evenly into the stirred Na2CO3 aqueous solution at a rate of 5 seconds per drop using a rubber-tipped dropper, and vigorously stir at a speed of 1600 rpm for 5 minutes to obtain a preliminarily mixed nitrate solution;

[0032] Step 4: Add dilute HNO3 dropwise to adjust the pH of the preliminarily mixed nitrate solution to 9;

[0033] Step 5: Monitor the pH value of the solution in real time and maintain the pH value of the solution at 9, and continue to stir vigorously at a speed of 1600 rpm for 30 minutes;

[0034] Step 6: Transfer the stirred solution to a 50 mL reactor, heat to 180°C, and keep warm for 500 minutes. After the reaction is completed, take out the precipitate in the reactor, wash it with high-purity water three times, and dry it at 50°C for 60 minutes to obtain the target product.

[0035] Example 2

[0036] Step 1: Take 1 g of each of a 0.3 mmol Gd(NO3)3·6H2O solution and a 0.7 mmol Tb(NO3)3·6H2O solution, mix the two, and obtain 2 g of a rare earth nitrate mixed solution;

[0037] Step 2: Take 20 g of Na2CO3 aqueous solution with a Na2CO3 content of 5 mmol and place it in a beaker containing a stirring bar for later use;

[0038] Step 3: Heat the Na2CO3 aqueous solution to 25°C, and drip the rare earth nitrate mixed solution evenly into the stirred Na2CO3 aqueous solution at a rate of 5 seconds per drop using a rubber-tipped dropper, and vigorously stir at a speed of 1600 rpm for 5 minutes to obtain a preliminarily mixed nitrate solution;

[0039] Step 4: Add dilute HNO3 dropwise to adjust the pH of the preliminarily mixed nitrate solution to 9;

[0040] Step 5: Monitor the pH value of the solution in real time and maintain the pH value of the solution at 9, and continue to stir vigorously at a speed of 1600 rpm for 30 minutes;

[0041] Step 6: Transfer the stirred solution to a 50 mL reactor, heat to 180 °C, and keep warm for 400 minutes;

[0042] Step 7: After the reaction is completed, take out the precipitate in the reactor, wash it with high-purity water three times, and dry it at 50°C for 60 minutes to obtain the target product.

[0043] Example 3

[0044] Step 1: Take 1 g of each of a 0.3 mmol Gd(NO3)3·6H2O solution and a 0.7 mmol Tb(NO3)3·6H2O solution, mix the two, and obtain 2 g of a rare earth nitrate mixed solution;

[0045] Step 2: Take 20 g of a 3 mmol Na2CO3 aqueous solution and place it in a beaker containing a stirring bar for later use;

[0046] Step 3: When the temperature of the Na2CO3 solution is 25°C, use a rubber-tipped dropper to evenly drop the rare earth nitrate mixed solution into the stirred Na2CO3 aqueous solution at a rate of 5 seconds per drop, and vigorously stir at a speed of 1600 rpm for 5 minutes;

[0047] Step 4: Add dilute HNO3 dropwise to adjust the pH of the preliminarily mixed nitrate solution to 9;

[0048] Step 5: Monitor the pH value of the solution in real time and continue to stir vigorously at 1600 rpm for 30 minutes, maintaining the pH value of the solution at 9 during stirring;

[0049] Step 6: Transfer the stirred solution to a 50 mL reactor, heat to 200°C, and keep warm for 500 minutes. After the reaction is completed, take out the precipitate in the reactor, wash it with high-purity water three times, and dry it at 50°C for 60 minutes to obtain the target product.

[0050] The physical structure of the obtained material was identified by X-ray diffractometer. Figure 1 As shown. Figure 1 As can be seen from the above, GOC:1Tb is prepared in the embodiment 3+ The diffraction peak position of the substance is completely consistent with Gd2O(CO3)2·H2O (JCPDS: 43-604) in the standard card library, and there is no other impurity phase, indicating that Tb in the lattice 3+ and Gd 3+ They can be substituted with each other in a high ratio and can maintain the consistency of the physical properties. Specifically, by comparing the preparation methods in Examples 1 and 2, it can be seen that the contents of Gd and Tb in the two examples are different and the reaction times are different. In the prepared product, GOC in Example 1: 0.5Tb 3+ and GOC in Example 2: 0.7 Tb 3+ , Tb in both materials 3+ The contents are 50% and 70% respectively, which are much greater than 17%. By comparing Example 2 and Example 3, it can be seen that when GOC: 0.7Tb is maintained 3+ Tb 3+ The content remains unchanged, but the amount of Na2CO3 in the reactant, the reaction temperature and the reaction time are changed to obtain Tb3+ However, in this method, the applicant has found through experiments that Na2CO3 cannot be directly replaced by alkali metal carbonates such as K2CO3 or Li2CO3.

[0051] Figure 2 From GOC: 1Tb 3+ It can be seen from the excitation spectrum that the excitation peaks of this substance have high excitation intensities at 254, 273, 283, 347 and 365 nm, and can be well excited by ultraviolet light of different wavelengths. Figure 3 Different Tb 3+ The emission spectrum of GOC with different doping concentrations under ultraviolet light excitation. From the emission intensity of fluorescence, it can be seen that with the increase of Tb 3+ As the doping concentration increases, the emission peak represented by the 541nm characteristic peak gradually increases, showing that Tb 3+ The higher the content, the stronger the fluorescence. 3+ The content reaches 70% (GOC: 1.4Tb 3+ ), and no fluorescence quenching phenomenon occurs. It can be seen that the method of the present invention successfully introduces a high concentration of Tb into the magnetic resonance material Gd2O(CO3)2·H2O. 3+ , realizing the preparation of dual imaging materials with both magnetic resonance and fluorescence in a single material.

[0052] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a material having dual imaging functions of fluorescence and magnetic resonance imaging, characterized in that: The general chemical formula of this material is Gd 2(1-x) O(CO3)2·H2O:2xTb 3+ , where x is Tb 3+ and (Tb 3+ +Gd 3+ ), 0 <x<0.8; The preparation method comprises the following steps: S1, absorb Gd(NO3)3 aqueous solution and Tb(NO3)3 aqueous solution in a certain proportion to obtain a metal nitrate mixed solution; S2. Take a certain amount of Na2CO3 aqueous solution and place it in a beaker containing a stirring bar for later use; S3, after heating the Na2CO3 aqueous solution to 15-30°C, use a rubber-tipped dropper to evenly drop the metal nitrate solution into the stirred Na2CO3 aqueous solution, and vigorously stir at a speed of 1600-2100 rpm for 5-10 minutes to obtain a nitrate solution; S4, adding dilute HNO3 dropwise to adjust the pH value of the nitrate solution; S5, monitor the pH value of the solution in real time and maintain the pH value of the solution, stirring vigorously for 30 minutes; S6. Transfer the stirred solution to a 50 mL reactor, heat to 170-220° C., and keep warm for 360-720 minutes. After the reaction is completed, take out the precipitate, wash it with high-purity water, and dry it to obtain the target product.

2. The method for preparing a material having dual imaging functions of fluorescence and magnetic resonance angiography according to claim 1, characterized in that : The metal nitrate solution contains Gd 3+ and Tb 3+ Two types of metal ions, and 0 <Tb 3+ / (Tb 3+ +Gd 3+ )<0.

8.

3. The method for preparing a material having dual imaging functions of fluorescence and magnetic resonance angiography according to claim 1, characterized in that : In the step S3, the molar ratio of Na2CO3 to metal nitrate is 2 to 8.

4. The method for preparing a material having dual imaging functions of fluorescence and magnetic resonance angiography according to claim 1, characterized in that During the reaction, the pH value of the solution is maintained at a constant value of 8 to 11.

5. The method for preparing a material having dual imaging functions of fluorescence and magnetic resonance angiography according to claim 1, characterized in that In step S3, the metal nitrate mixed solution is evenly dropped into the stirred Na2CO3 aqueous solution using a rubber-tipped dropper at a rate of 5 seconds per drop.

Citation Information

Patent Citations

  • Preparation method of trivalent terbium-doped gadolinium oxysulfide luminescent material and product and application of trivalent terbium-doped gadolinium oxysulfide luminescent material