A method for preparing a plexiglass solid dose meter
By using a combination of specific dyes and stabilizers in organic glass dosimeters, its stability and measurement precision in high-dose measurements are improved, solving the problem of poor stability of organic glass dosimeters in the existing technology, and achieving Efficient measurement under strong radiation fields.
Patent Information
- Application Number
- CN202410180261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-02-18
AI Technical Summary
It is difficult to ensure the stability of existing organic glass dosimeters in high-dose measurements, especially in applications with strong radiation fields. The types of radiochromic dyes are limited and the stability after irradiation is poor, which affects the measurement precision.
A combination of base material, radiochromic dye, initiator, light stabilizer, and heat stabilizer is used to prepare a plexiglass solid dosimeter through steps such as prepolymerization, vacuum defoaming, mold filling, low-temperature polymerization, and high-temperature polymerization. The radiochromic effect of solvent red/solvent orange/solvent yellow dyes, combined with light stabilizers and heat stabilizers, improves the stability and measurement precision of the dosimeter.
The storage stability of the organic glass dosimeter before and after irradiation is improved. The measurement accuracy is ≤2% in the dose range of 5-50kGy. It is suitable for high-dose measurement fields, such as radiation processing.
Smart Images

Figure CN118050766B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radiation dose meters, in particular to an organic glass solid dose meter and a preparation method thereof. Background Art
[0002] A radiation dosimeter is an instrument that measures the nuclear radiation dose received within a given time. Based on the temperature effect caused by the absorption of radiation energy by matter, the ionization effect and chemical effect of radiation on matter, and the various changes in the physical properties of solid matter, the measurement of radiation dose can be divided into calorimetry, ionization chamber method, chemical dosimetry and solid dosimeter. Solid dosimeter measures radiation dose by means of changes caused by certain solid materials (such as certain inorganic or organic crystals, glass and polymers, etc.) absorbing radiation energy. Solid dosimeters mainly include thermoluminescent dosimeters, film dosimeters, fluorescent glass dosimeters, track dosimeters, semiconductor dosimeters, etc. Because solid dosimeters can be made into thin sheets or films, they can be used to measure the dose distribution in samples. They are widely used in personal dose measurement, clinical dose measurement, environmental monitoring, radiobiology, radiation chemistry and radiation technology, reactor dose measurement and other fields.
[0003] At present, for the dose measurement of strong radiation fields, especially in the field of radiation processing, the widely used dosimeters are: liquid chemical dosimeters, radiochromic film dosimeters and plexiglass dosimeters. Liquid chemical dosimeters have high sensitivity, but their measurement process is relatively cumbersome and greatly affected by environmental factors; radiochromic film dosimeters and plexiglass dosimeters are simple to operate and easy to test, but the preparation process of film dosimeters is complicated, and there are very few radiochromic dyes suitable for plexiglass dosimeters, and their stability after irradiation is difficult to guarantee. Therefore, dosimeters suitable for high-dose measurement need to be developed. Summary of the invention
[0004] The object of the present invention is to provide a polymethyl methacrylate solid dosimeter and a preparation method thereof, so as to solve the problem that the above-mentioned dosimeter for high-dose measurement is difficult to ensure stability.
[0005] To achieve the above objectives, the first aspect of the present invention provides an organic glass solid dosimeter, which comprises, by weight, 100 parts of a substrate material, 0.02-0.05 parts of a radiation-chromic dye, 0.1-0.2 parts of an initiator, 0.2-0.5 parts of a light stabilizer, and 0.2-0.5 parts of a heat stabilizer.
[0006] Preferably, the substrate material is methyl methacrylate with a purity greater than 99.5% and containing 30 ppm DMBP stabilizer.
[0007] Preferably, the radiation-chromic dye is one or more of Solvent Red 135, Solvent Red 179, Solvent Red 195, Solvent Red 52, Solvent Red 23, Solvent Red 149, Solvent Orange 60, Solvent Orange 107, Solvent Yellow 179, Solvent Yellow 93, and Solvent Yellow 160, and the purity of the radiation-chromic dye is greater than 99.5%.
[0008] Solvent red / solvent orange / solvent yellow dyes have high thermal stability, light resistance and migration resistance. Under the irradiation of high-energy rays such as X / gamma and beta rays, the groups in the dyes undergo radiochemical reactions to generate new chromogenic groups. After irradiation, the color of the dosimeter darkens, and the degree of darkening is linearly related to the absorbed dose and can be quickly measured by spectrophotometry.
[0009] Preferably, the initiator is an azo initiator or a peroxide initiator.
[0010] Preferably, the initiator is benzoyl peroxide.
[0011] Preferably, the light stabilizer is one or more of benzotriazoles, salicylates, phosphites, and benzophenones.
[0012] Preferably, the light stabilizer is benzotriazole, which is used to absorb ultraviolet rays with a wavelength of 270-340nm and has a good light stabilization effect.
[0013] Preferably, the heat stabilizer is one or more of complex compounds, metal soaps, and basic lead salts.
[0014] Preferably, the heat stabilizer is a liquid calcium-zinc composite compound, the main components of which include calcium stearate, calcium ricinoleate, zinc stearate, zinc ricinoleate, and epoxy oil, which is used to inhibit thermal oxidative degradation reactions and delay or prevent the breakage and degradation of polymer molecular chains at high temperatures.
[0015] A second aspect of the present invention provides a method for preparing a plexiglass solid dosimeter, comprising the following steps:
[0016] 1) Prepolymerization: inject the substrate material into the reaction kettle, add the initiator, radiation color dye, light stabilizer and heat stabilizer in sequence, seal the reaction kettle and place it in a water bath for stirring and reaction, and when the solution viscosity reaches 500mPa·s, stop heating and quickly cool to room temperature to obtain a prepolymer;
[0017] 2) Vacuum defoaming: Open the reactor and place the prepolymer in a vacuum defoaming machine for vacuum defoaming;
[0018] 3) Mold pouring: pouring the prepolymer obtained in step (2) into a special glass mold, controlling the mold pouring thickness, and using a shaping pressure device to ensure uniform mold pouring thickness;
[0019] 4) Low temperature polymerization: The special glass mold after molding is placed in an oven for low temperature polymerization;
[0020] 5) High temperature polymerization: After the low temperature polymerization is completed, the mold is subjected to high temperature polymerization;
[0021] 6) Cooling and demolding: After the high-temperature polymerization is completed, it is naturally cooled to room temperature, and the special glass mold is removed to obtain the organic glass dosage sheet;
[0022] 7) Cutting and packaging: The plexiglass dose sheet is processed by a laser cutting machine to be made into a rectangular parallelepiped to obtain a plexiglass solid dose meter.
[0023] Preferably, in step (1), the water bath temperature is 90-95° C. and the stirring time is 20-25 min; in step (2), vacuum degassing is performed at 0.1 Pa for 15-20 min; and in step (3), a 3 mm diameter sealing ring is used to control the mold thickness.
[0024] Preferably, in step (4), the low-temperature polymerization is carried out at 50-70° C. for 18-24 hours.
[0025] Preferably, in step (5), high temperature polymerization is carried out at 100-120° C. for 2-4 hours.
[0026] Preferably, in step (7), a laser cutting machine is used to process the material into a cuboid of 30 mm×11 mm×3 mm.
[0027] Preferably, in step (7), the prepared organic glass solid dosimeter is packaged in an aluminum foil bag and sealed for storage.
[0028] Therefore, the present invention adopts a polymethyl methacrylate solid dosimeter with the above structure and a preparation method thereof, which has the following beneficial effects:
[0029] (1) The organic glass solid dosimeter prepared by the present invention utilizes the radiation colorization effect of solvent red / solvent orange / solvent yellow dyes and combines the use of light stabilizers and heat stabilizers to improve the storage stability of the organic glass dosimeter before and after irradiation.
[0030] (2) The organic glass solid dosimeter of the present invention has a good response within the dose range of 5-50 kGy, and a measurement precision of ≤2%. It can be used as a solid dosimeter in high-dose measurement fields such as radiation processing.
[0031] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a graph showing the color change of the dosimeter of Example 1 with the absorbed dose;
[0033] Figure 2 is the dosimeter dose response curve of Example 1;
[0034] Figure 3 This is a stability test diagram of the dosimeter of Example 1 before and after irradiation. DETAILED DESCRIPTION
[0035] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.
[0036] Example 1
[0037] A method for preparing a red organic glass solid dosimeter comprises the following steps:
[0038] 1) PMMA prepolymerization: 100 parts of methyl methacrylate as a substrate material was injected into a heating kettle, and 0.1 parts of benzoyl peroxide, 0.02 parts of solvent red 135, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex were added in sequence. The reaction kettle was sealed and placed in a 95°C water bath, and stirred electrically for 30 minutes. When the solution viscosity reached 500 mPa·s, heating was stopped and the solution was quickly cooled to room temperature to obtain a PMMA prepolymer;
[0039] 2) Vacuum defoaming: After the above steps are completed, open the reactor and place it in a vacuum defoaming machine for 20 minutes at 0.1 Pa;
[0040] 3) Mold pouring: The prepolymer obtained through the above steps is poured into a special glass mold, a 3mm diameter sealing ring is used to control the mold pouring thickness, and a shaping pressure device is used to ensure uniform mold pouring thickness;
[0041] 4) Low-temperature polymerization: The mold after molding is placed in a constant temperature oven and polymerized at 60°C for 4 hours;
[0042] 5) High temperature polymerization: After the low temperature polymerization is completed in the above steps, the mold is taken out and placed in a 120°C oven for high temperature polymerization for 2 hours;
[0043] 6) Cooling and demolding: After the high-temperature polymerization is completed in the above steps, the mold is taken out of the oven, cooled naturally to room temperature, and the mold is removed to obtain the organic glass dosage sheet;
[0044] 7) Cutting and packaging: The organic glass dosage sheet obtained by demolding is processed by a laser cutting machine to obtain a 30 mm × 11 mm × 3 mm rectangular parallelepiped, that is, a red organic glass solid dosimeter, which is sealed in an aluminum foil bag for storage.
[0045] Example 2
[0046] A method for preparing a red organic glass solid dosimeter comprises the following steps:
[0047] 1) PMMA prepolymerization: 100 parts of methyl methacrylate as a substrate material was injected into a heating kettle, and 0.1 parts of benzoyl peroxide, 0.02 parts of solvent red 179, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex were added in sequence. The reaction kettle was sealed and placed in a 95°C water bath, and stirred electrically for 30 minutes. When the solution viscosity reached 500 mPa·s, heating was stopped and the solution was quickly cooled to room temperature to obtain a PMMA prepolymer;
[0048] 2) Vacuum defoaming: After the above steps are completed, open the reactor and place it in a vacuum defoaming machine for 20 minutes at 0.1 Pa;
[0049] 3) Mold pouring: The prepolymer obtained through the above steps is poured into a special glass mold, a 3mm diameter sealing ring is used to control the mold pouring thickness, and a shaping pressure device is used to ensure uniform mold pouring thickness;
[0050] 4) Low-temperature polymerization: The mold after molding is placed in a constant temperature oven and polymerized at 60°C for 4 hours;
[0051] 5) High temperature polymerization: After the low temperature polymerization is completed in the above steps, the mold is taken out and placed in a 120°C oven for high temperature polymerization for 2 hours;
[0052] 6) Cooling and demolding: After the high-temperature polymerization is completed in the above steps, the mold is taken out of the oven, cooled naturally to room temperature, and the mold is removed to obtain the organic glass dosage sheet;
[0053] 7) Cutting and packaging: The organic glass dosage sheet obtained by demolding is processed by a laser cutting machine to obtain a 30 mm × 11 mm × 3 mm rectangular parallelepiped, that is, a red organic glass solid dosimeter, which is sealed in an aluminum foil bag for storage.
[0054] Example 3
[0055] A method for preparing a red organic glass solid dosimeter comprises the following steps:
[0056] 1) PMMA prepolymerization: 100 parts of methyl methacrylate as a substrate material was injected into a heating kettle, and 0.1 parts of benzoyl peroxide, 0.02 parts of solvent red 195, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex were added in sequence. The reaction kettle was sealed and placed in a 95°C water bath, and stirred electrically for 30 minutes. When the solution viscosity reached 500 mPa·s, heating was stopped and the solution was quickly cooled to room temperature to obtain a PMMA prepolymer;
[0057] 2) Vacuum defoaming: After the above steps are completed, open the reactor and place it in a vacuum defoaming machine for 20 minutes at 0.1 Pa;
[0058] 3) Mold pouring: The prepolymer obtained through the above steps is poured into a special glass mold, a 3mm diameter sealing ring is used to control the mold pouring thickness, and a shaping pressure device is used to ensure uniform mold pouring thickness;
[0059] 4) Low-temperature polymerization: The mold after molding is placed in a constant temperature oven and polymerized at 60°C for 4 hours;
[0060] 5) High temperature polymerization: After the low temperature polymerization is completed in the above steps, the mold is taken out and placed in a 120°C oven for high temperature polymerization for 2 hours;
[0061] 6) Cooling and demolding: After the high-temperature polymerization is completed in the above steps, the mold is taken out of the oven, cooled naturally to room temperature, and the mold is removed to obtain the organic glass dosimeter;
[0062] 7) Cutting and packaging: The organic glass dosage sheet obtained by demolding is processed by a laser cutting machine to obtain a 30 mm × 11 mm × 3 mm rectangular parallelepiped, that is, a red organic glass solid dosimeter, which is sealed in an aluminum foil bag for storage.
[0063] Example 4
[0064] A method for preparing an orange organic glass solid dosimeter comprises the following steps:
[0065] 1) PMMA prepolymerization: 100 parts of methyl methacrylate as a substrate material was injected into a heating kettle, and 0.1 parts of benzoyl peroxide, 0.02 parts of solvent orange 60, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex were added in sequence. The reaction kettle was sealed and placed in a 95°C water bath, and stirred electrically for 30 minutes. When the solution viscosity reached 500 mPa·s, heating was stopped and the solution was quickly cooled to room temperature to obtain a PMMA prepolymer;
[0066] 2) Vacuum defoaming: After the above steps are completed, open the reactor and place it in a vacuum defoaming machine for 20 minutes at 0.1 Pa;
[0067] 3) Mold pouring: The prepolymer obtained through the above steps is poured into a special glass mold, a 3mm diameter sealing ring is used to control the mold pouring thickness, and a shaping pressure device is used to ensure uniform mold pouring thickness;
[0068] 4) Low-temperature polymerization: The mold after molding is placed in a constant temperature oven and polymerized at 60°C for 4 hours;
[0069] 5) High temperature polymerization: After the low temperature polymerization is completed in the above steps, the mold is taken out and placed in a 120°C oven for high temperature polymerization for 2 hours;
[0070] 6) Cooling and demolding: After the high-temperature polymerization is completed in the above steps, the mold is taken out of the oven, cooled naturally to room temperature, and the mold is removed to obtain the organic glass dosage sheet;
[0071] 7) Cutting and packaging: The organic glass dosage sheet obtained by demolding is processed by a laser cutting machine to obtain a 30 mm×11 mm×3 mm rectangular parallelepiped, that is, the orange organic glass solid dosage meter is obtained, which is sealed in an aluminum foil bag for storage.
[0072] Example 5
[0073] A method for preparing a yellow organic glass solid dosimeter comprises the following steps:
[0074] 1) PMMA prepolymerization: 100 parts of methyl methacrylate, a substrate material, were injected into a heating kettle, and 0.1 parts of benzoyl peroxide, 0.02 parts of solvent yellow 179, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex were added in sequence. The reaction kettle was sealed and placed in a 95°C water bath, and stirred electrically for 30 minutes. When the solution viscosity reached 500 mPa·s, heating was stopped and the solution was quickly cooled to room temperature to obtain a PMMA prepolymer;
[0075] 2) Vacuum defoaming: After the above steps are completed, open the reactor and place it in a vacuum defoaming machine for 20 minutes at 0.1 Pa;
[0076] 3) Mold pouring: The prepolymer obtained through the above steps is poured into a special glass mold, a 3mm diameter sealing ring is used to control the mold pouring thickness, and a shaping pressure device is used to ensure uniform mold pouring thickness;
[0077] 4) Low-temperature polymerization: The mold after molding is placed in a constant temperature oven and polymerized at 60°C for 4 hours;
[0078] 5) High temperature polymerization: After the low temperature polymerization is completed in the above steps, the mold is taken out and placed in a 120°C oven for high temperature polymerization for 2 hours;
[0079] 6) Cooling and demolding: After the high-temperature polymerization is completed in the above steps, the mold is taken out of the oven, cooled naturally to room temperature, and the mold is removed to obtain the organic glass dosage sheet;
[0080] 7) Cutting and packaging: The organic glass dosage sheet obtained by demoulding is processed by a laser cutting machine to obtain a 30 mm×11 mm×3 mm rectangular parallelepiped, that is, the yellow organic glass solid dosimeter is obtained, which is sealed in an aluminum foil bag for storage.
[0081] Comparative Example 1
[0082] The difference from Example 1 is that the prepolymerization in step (1) is omitted, and 100 parts of methyl methacrylate as a substrate material, 0.1 parts of benzoyl peroxide, 0.02 parts of solvent red 135, 0.2 parts of benzotriazole and 0.2 parts of liquid calcium zinc complex are added in sequence to form a mixture, and the mixture is directly subjected to the vacuum degassing step.
[0083] Comparative Example 2
[0084] The difference from Example 1 is that step (4) of low-temperature polymerization is omitted, and the high-temperature polymerization step is directly performed after molding.
[0085] Comparative Example 3
[0086] The difference from Example 1 is that the step (5) of high-temperature polymerization is omitted, and the molding is directly performed by cooling and demoulding after low-temperature polymerization.
[0087] Test example
[0088] The spectrophotometric method was used to test the dose response performance of the organic glass solid dosimeter. The specific experimental method is as follows: the organic glass solid dosimeter irradiated with different doses is placed in the spectrophotometer measurement chamber to measure its absorbance A, and the absorbance per centimeter APC is calculated by the ratio of absorbance A to the thickness of the dosimeter d (cm) = A / d (cm -1 ).
[0089] Figure 1 The color change diagram of the red organic glass solid dosimeter obtained in Example 1 with the irradiation dose is shown in FIG. Figure 1 It can be seen that as the absorbed dose increases, the color of the red plexiglass solid dosimeter gradually becomes darker. Figure 2 is the dose response curve of the dosimeter, from Figure 2 It can be seen that the relationship between absorbed dose and absorbance per centimeter is: y = 5 × 10 -5 x 3 -0.0057x 2 +0.2293x-0.1509, R 2 =0.9954, the correlation coefficient between the absorbance per unit thickness (APC) of the dosimeter and the irradiated dose (R 2 ) is greater than 0.995, indicating that the prepared dosimeter has excellent dose response performance. Figure 3 is the change of the absorbance of the dosimeter with time before and after irradiation. Figure 3 It can be seen that the dosimeter has good stability before and after irradiation. The absorbance before irradiation does not change with storage time, and the absorbance change after 10 days of irradiation is less than 4%.
[0090] The absorbance changes of the dosimeters prepared in Example 1 and Comparative Examples 1-3 before and after irradiation were tested. The test results are shown in Table 1.
[0091] Table 1 Absorbance change results of the dosimeters prepared in Example 1 and Comparative Examples 1-3 before and after irradiation
[0092]
[0093] Therefore, the present invention adopts the above-mentioned organic glass solid dosimeter and its preparation method. The prepared organic glass solid dosimeter utilizes the radiation colorization effect of solvent red / solvent orange / solvent yellow dyes, and combines the use of light stabilizers and heat stabilizers to improve the storage stability of the organic glass dosimeter before and after irradiation. The organic glass solid dosimeter responds well within the dose range of 5-50kGy, and the measurement precision is ≤2%. It can be used as a solid dosimeter in high-dose measurement fields such as radiation processing.
[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a plexiglass solid dosimeter, Features: The following steps are involved: 1) Prepolymerization: inject the substrate material into the reaction kettle, add the initiator, radiation color dye, light stabilizer and heat stabilizer in sequence, seal the reaction kettle and place it in a water bath for stirring and reaction, and when the solution viscosity reaches 500mPa·s, stop heating and quickly cool to room temperature to obtain a prepolymer; The organic glass solid dosimeter includes 100 parts of base material, 0.02 parts of radiation coloring dye, 0.1 parts of initiator, 0.2 parts of light stabilizer and 0.2 parts of heat stabilizer according to weight parts; The base material is methyl methacrylate with a purity greater than 99.5% and contains 30ppm DMBP stabilizer; The radiation-induced color dye is one of solvent red 135, solvent red 179, solvent red 195, solvent orange 60, and solvent yellow 179, and the purity of the radiation-induced color dye is greater than 99.5%; The initiator is benzoyl peroxide; The light stabilizer is benzotriazole; The heat stabilizer is a liquid calcium-zinc complex; 2) Vacuum defoaming: Open the reactor and place the prepolymer in a vacuum defoaming machine for vacuum defoaming; 3) Mold pouring: pouring the prepolymer obtained in step (2) into a special glass mold, controlling the mold pouring thickness, and using a shaping pressure device to ensure uniform mold pouring thickness; 4) Low temperature polymerization: The special glass mold after molding is placed in an oven for low temperature polymerization; 5) High temperature polymerization: After the low temperature polymerization is completed, the mold is subjected to high temperature polymerization; 6) Cooling and demolding: After the high-temperature polymerization is completed, it is naturally cooled to room temperature, and the special glass mold is removed to obtain the organic glass dosage sheet; 7) Cutting and packaging: The plexiglass dose sheet is processed by a laser cutting machine to be made into a rectangular parallelepiped to obtain a plexiglass solid dose meter.
2. A method for preparing a polymethyl methacrylate solid dosimeter according to claim 1, Features: In step (1), the water bath temperature is 90-95° C. and the stirring time is 20-25 min. In step (2), vacuum degassing is performed at 0.1 Pa for 15-20 min. In step (3), a 3 mm diameter sealing ring is used to control the mold thickness.
3. The method for preparing a plexiglass solid dosimeter according to claim 1, Features: In step (4), low temperature polymerization is carried out at 50-70° C. for 18-24 hours.
4. The method for preparing a plexiglass solid dosimeter according to claim 1, Features: In step (5), high temperature polymerization is carried out at 100-120° C. for 2-4 hours.