A process for removing impurities from multi-component brightening agent
Through the surface modification treatment of nano SiO2 and the use of hydrophilic modified ultrafiltration membrane, the problem of nano-silicon dioxide agglomeration in the polishing agent is solved, the polishing efficiency and quality are improved, and a more efficient polishing effect is achieved.
Patent Information
- Application Number
- CN202410432100.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-11
AI Technical Summary
Nanosilicon dioxide is prone to agglomeration in the polishing agent due to its small particle size and large specific surface area, resulting in inconsistent polishing quality and reduced polishing efficiency.
NanoSiO2 was modified with 3-aminopropyltriethoxysilane, and filtration was used for removal of impurities using a hydrophilic modified ultrafiltration membrane to reduce agglomeration phenomenon, improve dispersion stability and polishing efficiency.
Through the combination of modification treatment and filtration and impurities removal, the dispersion stability and compatibility of nano SiO2 are significantly improved, unstable agglomerates and impurities are removed, ensuring the efficiency and high quality of the polishing agent, and improving the polishing efficiency and Effect.
Smart Images

Figure CN118059681B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultrafiltration membrane impurity removal, and in particular relates to a multi-component brightening agent impurity removal process method. Background Art
[0002] Polishing agents, also known as brighteners, have the function of making the surface bright. Polishing agents are usually used to clean and increase the gloss of metal surfaces. Such products do not contain harmful additives such as sulfur, phosphorus, and chlorine. They can not only effectively remove oil stains, prevent rust, and clean metals, but also make metal products reveal the true metallic luster. In actual applications, the metal surface after using water-soluble polishes is usually smoother and brighter, thus achieving the effect of "brightening".
[0003] CN104059539A discloses a high-efficiency diamond polishing agent and a preparation method thereof. The surface of diamond micropowder is modified by using ethyl orthosilicate to form a silicon dioxide coating layer on the surface of the diamond micropowder. The coating layer can play a buffering role on the inner layer of diamond micropowder during polishing. The morphology of the diamond micropowder is made closer to an iso-octahedron by repeatedly crushing and shaping the diamond micropowder and improving the surface modification process. The polishing agent prepared not only has a good polishing effect on high-hardness metal materials such as high-carbon steel, but also has a good polishing effect on Cr 2 O 3 , ceramics, jade, quartz and other hard and brittle materials also have good polishing effects. However, due to its extremely fine particle size and high surface energy, diamond powder is still very easy to agglomerate even if a silicon dioxide coating is formed on the surface, which affects the uniform distribution of abrasive particles and reduces polishing efficiency and quality.
[0004] CN101838503A discloses a polishing agent for renovation of polished bricks, stone materials, and artificial stones. The polishing agent is configured by adding a fluorine-containing additive, a pH regulator, and other additives to one or more nano-silicon dioxide. Unlike general polishing agents, it can not only remove dirt on the surface of bricks, but also restore the color of polished bricks, marble, granite, artificial stones, etc., and the durability can be significantly improved, and it is even more luxurious and beautiful than new floor decoration. However, the small size and large specific surface area of nano-silicon dioxide make them tend to attract each other through van der Waals forces and other intermolecular forces, thereby forming agglomerates, resulting in inconsistent polishing quality and reduced polishing efficiency. Summary of the invention
[0005] In order to solve the problems existing in the background technology, the present invention provides a multi-component brightener impurity removal process method, which synergistically reduces the agglomeration phenomenon and improves the polishing efficiency through surface modification of nanoparticles and targeted filtering and impurity removal.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A multi-component brightener impurity removal process method comprises the following steps:
[0008] S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 ;
[0009] S2, by weight, 10 parts of the modified nano-SiO 2 Dispersed in 35-50 parts of deionized water to obtain dispersed particle liquid;
[0010] S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO 2 , and obtain impurity particle removal liquid;
[0011] S4, centrifugally separate the impurity-removed particle liquid obtained in S3, and vacuum dry it to obtain purified modified SiO 2 ;
[0012] S5, by weight, 1-2 parts of an oxidant, 2-3 parts of a stabilizer, 2-3 parts of a chelating agent, 10-15 parts of a wetting agent, 28-35 parts of deionized water and 30 parts of the purified modified SiO obtained in S4 2 Mix well to obtain a multi-component brightener.
[0013] Further, in S1, the modified nano-SiO 2 The specific preparation steps are as follows:
[0014] A1. 40g of nano-SiO 2 Add into 1000 mL of toluene and disperse by ultrasonic at room temperature for 30 min to obtain a suspension;
[0015] A2, adding 18.2 g of 3-aminopropyltriethoxysilane to the suspension obtained in A1, and ultrasonically dispersing at room temperature for 5 min to obtain a dispersion;
[0016] A3, transfer the dispersion obtained in A2 into a thermostatic bath, and react at 90°C for 6 hours to obtain a reaction solution;
[0017] A4, centrifuge the reaction solution obtained in A3, and vacuum dry it to obtain modified nano-SiO 2 .
[0018] Furthermore, the nano-SiO 2 The particle size is 10-40nm.
[0019] Furthermore, in both A1 and A2, a 300W ultrasonic cleaner was used for ultrasonic dispersion.
[0020] Furthermore, S4 and A4 were both centrifuged at 12000 r / min at room temperature.
[0021] Further, the specific operation steps of S2 are as follows: weigh 10 parts by weight of modified nano-SiO 2 and 35-50 parts of deionized water, and weigh the modified nano-SiO 2 Slowly add it into deionized water and stir it with a magnetic stirrer at a speed of 500-800 rpm for 0.5-2 h to obtain a dispersed particle liquid.
[0022] Furthermore, the preparation method of the hydrophilic modified ultrafiltration membrane is as follows:
[0023] B1. Mix 15-25 parts of polysulfone, 70-80 parts of N,N-dimethylacetamide, 3-5 parts of polyvinyl pyrrolidone and 4-7 parts of acrylamide by weight, and mechanically stir at 60°C for 6-8h to obtain a hydrophilic casting solution;
[0024] B2. After the hydrophilic casting liquid obtained in B1 is allowed to stand and degas at room temperature for 24 hours, it is poured onto a glass plate and scraped with a scraper at a uniform speed to form a liquid film of uniform thickness. It is then quickly placed in a deionized water coagulation bath. When the film layer completely and autonomously detaches from the glass plate, a hydrophilic modified ultrafiltration membrane is obtained.
[0025] Furthermore, the oxidant is hydrogen peroxide, and the stabilizer is ferrous chloride.
[0026] Furthermore, the chelating agent includes ethylenediaminetetraacetic acid and / or nitrilotriacetic acid.
[0027] Furthermore, the wetting agent includes stearic acid and acetone, and the mass ratio of the two is 2:3-4.
[0028] This application has the following beneficial effects:
[0029] 1. The present invention uses 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification is performed to improve its dispersion stability in the polishing agent, reduce the agglomeration of particles, and allow more effective abrasive particles to participate in the polishing process, thereby improving the polishing efficiency; the hydrophilic modified ultrafiltration membrane is used for filtration and impurity removal, effectively intercepting the unmodified nano-SiO 2 , remove impurities that affect polishing efficiency and effect; the combination of modification treatment and filtration and impurity removal not only improves the quality of nano-SiO 2 It improves the dispersion stability and compatibility, and removes unstable agglomerates and impurities. This double optimization ensures the high efficiency and high quality of the polishing agent.
[0030] 2. Modified Nano-SiO 2 During the preparation, nano-SiO2 Adding toluene and dispersing by ultrasound can help break up the particles, reduce the original aggregation state, and facilitate the subsequent modification effect; 3-aminopropyltriethoxysilane and nano-SiO 2 Chemical reactions occur on the surface to form stable chemical bonds, improve the dispersion and stability of the particles in water, and make the particle surface more hydrophilic, which is crucial to prevent the particles from reaggregating and maintaining stability during the polishing process.
[0031] 3. In the preparation of hydrophilic modified ultrafiltration membrane, polysulfone, N,N-dimethylacetamide, polyvinyl pyrrolidone and acrylamide are selected. Among them, polysulfone is a commonly used membrane material with good mechanical properties and chemical stability. N,N-dimethylacetamide is used as a solvent to help dissolve the polymer, and polyvinyl pyrrolidone and acrylamide increase the hydrophilicity of the membrane. The increased hydrophilicity of the membrane surface can attract more water molecules to form a hydration layer, which helps to reduce the adsorption of pollutants on the membrane surface and reduce the possibility of membrane pollution. At the same time, the hydrophilic membrane has better permeability to water molecules, which helps to increase the water flux of the membrane. Based on the hydration layer and high water flux of the hydrophilic modified ultrafiltration membrane, the unmodified nano-SiO 2 Due to the lack of hydrophilic surface, it is easier to aggregate and deposit on the membrane surface, improving the interception efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A trend chart comparing the polishing efficiency of the multi-component brighteners prepared in Examples 1-8 of the present invention and Comparative Examples 1-5 on copper plates and 304 stainless steel, respectively;
[0033] Figure 2 The following is a trend chart comparing the polishing effects of the multi-component brighteners prepared in Examples 1-8 of the present invention and Comparative Examples 1-5 on copper plates and 304 stainless steel, respectively. DETAILED DESCRIPTION
[0034] The present application is further described in detail below with reference to the embodiments.
[0035] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0036] Embodiment 1: A multi-component brightener impurity removal process method, comprising the following steps:
[0037] S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 .
[0038] Modified Nano-SiO 2 The specific preparation steps are as follows:
[0039] A1. 40g of nano-SiO 2 Add to 1000mL toluene, nano-SiO 2 The particle size is 20 nm. At room temperature, ultrasonic dispersion is performed using a 300W ultrasonic cleaning apparatus for 30 minutes to obtain a suspension.
[0040] A2. Add 18.2 g of 3-aminopropyltriethoxysilane to the suspension obtained in A1, and perform ultrasonic dispersion for 5 min at room temperature using a 300 W ultrasonic cleaner to obtain a dispersion.
[0041] A3. Transfer the dispersion obtained in A2 into a thermostatic bath and react at 90°C for 6 hours to obtain a reaction solution.
[0042] A4. At room temperature, the reaction solution obtained in A3 was centrifuged at 12000r / min and vacuum dried to obtain modified nano-SiO 2 .
[0043] Among them, nano-SiO 2 Purchased from Nanjing Hongde Nanomaterial Co., Ltd.; particle size 20nm; purity 99+%; specific surface area 120m 2 / g; pH value is 5.5-6.5; the surface itself is hydrophilic. Due to its tiny particle size and large specific surface area, large surface energy and strong surface adsorption, it is still easy to spontaneously aggregate and agglomerate in the polishing liquid.
[0044] 3-Aminopropyltriethoxysilane (Kramar) was purchased from Shanghai Puzhen Biotechnology Co., Ltd. 2 Surface modification to increase hydrophilicity can help reduce the occurrence of agglomeration.
[0045] S2, weigh 10 parts of modified nano-SiO 2 and 45 parts of deionized water, and the weighed modified nano-SiO 2 Slowly add deionized water to avoid agglomeration due to rapid addition; stir with a magnetic stirrer at a speed of about 700 rpm for 1.2 hours to obtain dispersed particle liquid. This operation should be performed under dust-free or well-controlled conditions to prevent impurities from mixing in.
[0046] S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO 2 , and obtain the impurity particle removal liquid.
[0047] The specific operation is as follows: First, install the hydrophilic modified ultrafiltration membrane in the plate membrane laboratory filtration equipment model bona-gm-040, ensure that the membrane surface is flat and well sealed to prevent solution leakage. Check whether the pipeline of the ultrafiltration system is unobstructed, ensure that all connections are leak-free, and perform a pressure test on the system. Before the formal filtration, pre-filter the membrane with deionized water to remove possible contaminants remaining on the membrane surface and check the integrity of the membrane. Then, pour the dispersed particle liquid into the filtration equipment, operate at a pressure of 0.4MPa, and at room temperature to start filtration.
[0048] Wherein, the preparation method of the hydrophilic modified ultrafiltration membrane is as follows:
[0049] B1. Mix 20 parts of polysulfone, 75 parts of N,N-dimethylacetamide, 4 parts of polyvinyl pyrrolidone and 5 parts of acrylamide by weight, and stir mechanically at 60°C for 6-8h to obtain a hydrophilic casting solution.
[0050] Among them, polysulfone (US Solvay) was purchased from Dongguan Maoke Plastic Raw Materials Co., Ltd., which is used as a membrane material and is the main component of ultrafiltration membrane. N,N-dimethylacetamide was purchased from Jinan Ronghui Chemical Co., Ltd., and the quality standard implemented is the national standard. The content is 99.95%. It is used as a solvent to dissolve polysulfone and other additives. Polyvinylpyrrolidone was purchased from Guangdong Yuemei Chemical Co., Ltd., which is used as a porogen and stabilizer to help form membrane pores and maintain the stability of the casting liquid. Acrylamide was purchased from Shanghai Gaoming Chemical Co., Ltd., with a content of 99.8%. It can be used as a cross-linking agent / functional monomer to introduce hydrophilic groups and enhance the hydrophilicity of the membrane.
[0051] B2. The hydrophilic casting liquid obtained in B1 is allowed to stand at room temperature for 24 hours to remove bubbles and prevent defects during film formation. Then pour it onto a glass plate and use a scraper to scrape it into a liquid film of uniform thickness at a uniform speed. During the specific operation, the thickness of the liquid film is controlled to be 200 μm by adjusting the distance between the scraper and the glass plate. When using the scraper, keep moving at a uniform speed and apply uniform pressure to ensure that the thickness of the film layer is consistent. After scraping the film, quickly put it into a deionized water coagulation bath. When the film layer completely detaches from the glass plate autonomously, it indicates that the film has been formed and has sufficient strength and integrity, and a hydrophilic modified ultrafiltration membrane is obtained.
[0052] S4, at room temperature, centrifuge the impurity-removing particle liquid obtained in S3 at 12000r / min, and vacuum dry to obtain purified modified SiO 2 .
[0053] S5, by weight, 1.5 parts of oxidant, 2.5 parts of stabilizer, 2.5 parts of chelating agent, 13 parts of wetting agent, 33 parts of deionized water and 30 parts of purified modified SiO obtained in S4 were mixed. 2 Mix well to obtain a multi-component brightener.
[0054] The oxidant is hydrogen peroxide, the stabilizer is ferrous chloride, the chelating agent includes ethylenediaminetetraacetic acid and nitrilotriacetic acid, and the mass ratio of the two is 1:2, and the wetting agent includes stearic acid and acetone, and the mass ratio of the two is 2:3.
[0055] Example 2: The difference between this example and Example 1 is that in the preparation of the hydrophilic modified ultrafiltration membrane, the raw material components of the hydrophilic membrane casting solution are different.
[0056] Specifically, the preparation method of the hydrophilic modified ultrafiltration membrane is as follows:
[0057] B1. Mix 15 parts of polysulfone, 70 parts of N,N-dimethylacetamide, 3 parts of polyvinyl pyrrolidone and 4 parts of acrylamide by weight, and stir mechanically at 60°C for 6-8h to obtain a hydrophilic casting solution.
[0058] B2. The hydrophilic casting liquid obtained in B1 is allowed to stand at room temperature for 24 hours to remove bubbles and prevent defects during film formation. Then pour it onto a glass plate and use a scraper to scrape it into a liquid film of uniform thickness at a uniform speed. During the specific operation, the thickness of the liquid film is controlled to be 200 μm by adjusting the distance between the scraper and the glass plate. When using the scraper, keep moving at a uniform speed and apply uniform pressure to ensure that the thickness of the film layer is consistent. After scraping the film, quickly put it into a deionized water coagulation bath. When the film layer completely detaches from the glass plate autonomously, it indicates that the film has been formed and has sufficient strength and integrity, and a hydrophilic modified ultrafiltration membrane is obtained.
[0059] Example 3: The only difference between this example and Example 1 is that in the preparation of the hydrophilic modified ultrafiltration membrane, the raw material components of the hydrophilic casting solution are different.
[0060] Specifically, the preparation method of the hydrophilic modified ultrafiltration membrane is as follows:
[0061] B1. Mix 25 parts of polysulfone, 80 parts of N,N-dimethylacetamide, 5 parts of polyvinyl pyrrolidone and 7 parts of acrylamide by weight, and stir mechanically at 60°C for 6-8 hours to obtain a hydrophilic casting solution.
[0062] B2. The hydrophilic casting liquid obtained in B1 is allowed to stand at room temperature for 24 hours to remove bubbles and prevent defects during film formation. Then pour it onto a glass plate and use a scraper to scrape it into a liquid film of uniform thickness at a uniform speed. During the specific operation, the thickness of the liquid film is controlled to be 200 μm by adjusting the distance between the scraper and the glass plate. When using the scraper, keep moving at a uniform speed and apply uniform pressure to ensure that the thickness of the film layer is consistent. After scraping the film, quickly put it into a deionized water coagulation bath. When the film layer completely detaches from the glass plate autonomously, it indicates that the film has been formed and has sufficient strength and integrity, and a hydrophilic modified ultrafiltration membrane is obtained.
[0063] Embodiment 4: This embodiment differs from Embodiment 1 only in that: in S5, the raw material components of the multi-component brightener are different.
[0064] Specifically, a multi-component brightener impurity removal process method comprises the following steps:
[0065] S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 .
[0066] S2, weigh 10 parts of modified nano-SiO 2 and 45 parts of deionized water, and the weighed modified nano-SiO 2 Slowly add deionized water to avoid agglomeration due to rapid addition; stir with a magnetic stirrer at a speed of about 700 rpm for 1.2 hours to obtain dispersed particle liquid. This operation should be performed under dust-free or well-controlled conditions to prevent impurities from mixing in.
[0067] S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO 2 , and obtain the impurity particle removal liquid.
[0068] S4, at room temperature, centrifuge the impurity-removing particle liquid obtained in S3 at 12000r / min, and vacuum dry to obtain purified modified SiO 2 .
[0069] S5, by weight, 1 part of oxidant, 2 parts of stabilizer, 2 parts of chelating agent, 10 parts of wetting agent, 28 parts of deionized water and 30 parts of purified modified SiO obtained in S4 were mixed. 2 Mix well to obtain a multi-component brightener.
[0070] Embodiment 5: This embodiment differs from Embodiment 1 only in that: in S5, the raw material components of the multi-component brightener are different.
[0071] Specifically, a multi-component brightener impurity removal process method comprises the following steps:
[0072] S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 .
[0073] S2, weigh 10 parts of modified nano-SiO 2 and 45 parts of deionized water, and the weighed modified nano-SiO 2Slowly add deionized water to avoid agglomeration due to rapid addition; stir with a magnetic stirrer at a speed of about 700 rpm for 1.2 hours to obtain dispersed particle liquid. This operation should be performed under dust-free or well-controlled conditions to prevent impurities from mixing in.
[0074] S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO 2 , and obtain the impurity particle removal liquid.
[0075] S4, at room temperature, centrifuge the impurity-removing particle liquid obtained in S3 at 12000r / min, and vacuum dry to obtain purified modified SiO 2 .
[0076] S5, by weight, 2 parts of oxidant, 3 parts of stabilizer, 3 parts of chelating agent, 15 parts of wetting agent, 35 parts of deionized water and 30 parts of purified modified SiO obtained in S4 were mixed. 2 Mix well to obtain a multi-component brightener.
[0077] Example 6: The difference between this example and Example 1 is that in S5, the raw material components of the multi-component brightener are different.
[0078] Specifically, a multi-component brightener impurity removal process method comprises the following steps:
[0079] S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 .
[0080] S2, weigh 10 parts of modified nano-SiO 2 and 45 parts of deionized water, and the weighed modified nano-SiO 2 Slowly add deionized water to avoid agglomeration due to rapid addition; stir with a magnetic stirrer at a speed of about 700 rpm for 1.2 hours to obtain dispersed particle liquid. This operation should be performed under dust-free or well-controlled conditions to prevent impurities from mixing in.
[0081] S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO 2 , and obtain the impurity particle removal liquid.
[0082] S4, at room temperature, centrifuge the impurity-removing particle liquid obtained in S3 at 12000r / min, and vacuum dry to obtain purified modified SiO 2 .
[0083] S5, by weight, 1 part of oxidant, 2 parts of stabilizer, 3 parts of chelating agent, 10 parts of wetting agent, 35 parts of deionized water and 30 parts of purified modified SiO obtained in S4 were mixed. 2 Mix well to obtain a multi-component brightener.
[0084] Embodiment 7: This embodiment differs from Embodiment 1 only in that ethylenediaminetetraacetic acid is used as the chelating agent.
[0085] Embodiment 8: This embodiment differs from Embodiment 1 only in that the chelating agent is nitrilotriacetic acid.
[0086] Comparative Example 1: The difference between this comparative example and Example 1 is that the hydrophilic modified ultrafiltration membrane is replaced by a common ultrafiltration membrane.
[0087] Specifically, in S3, the dispersed particle liquid obtained in S2 is filtered using a common ultrafiltration membrane to obtain a particle liquid without impurities.
[0088] The preparation method of ordinary ultrafiltration membrane is as follows:
[0089] B1. Mix 20 parts of polysulfone, 75 parts of N,N-dimethylacetamide and 4 parts of polyvinylpyrrolidone by weight, and stir mechanically at 60°C for 6-8 hours to obtain a casting solution.
[0090] B2. The casting liquid obtained in B1 was allowed to stand at room temperature for 24 hours to degas. The liquid was poured onto a glass plate and scraped at a constant speed to form a liquid film of uniform thickness of 200 μm. The film was then quickly placed in a deionized water coagulation bath. When the film layer completely separated from the glass plate, a common ultrafiltration membrane was obtained.
[0091] Comparative Example 2: The difference between this comparative example and Example 1 is that the impurity removal step of the hydrophilic modified ultrafiltration membrane is directly deleted.
[0092] Specifically, S1, using 3-aminopropyltriethoxysilane to treat nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2 .
[0093] S2, by weight, 1.5 parts of oxidant, 2.5 parts of stabilizer, 2.5 parts of chelating agent, 13 parts of wetting agent, 33 parts of deionized water and 30 parts of modified nano-SiO obtained in S1 were mixed. 2 Mix well to obtain a multi-component brightener.
[0094] Comparative Example 3: The difference between this comparative example and Example 1 is that the purified modified SiO 2 Replaced with nano-SiO 2 ; That is, in the raw material components of the multi-component brightener, commercially available nano-SiO 2 , without modification or ultrafiltration to remove impurities.
[0095] Specifically, by weight, 1.5 parts of an oxidant, 2.5 parts of a stabilizer, 2.5 parts of a chelating agent, 13 parts of a wetting agent, 33 parts of deionized water and 30 parts of nano-SiO 2 Mix well to obtain a multi-component brightener.
[0096] Comparative Example 4: The difference between this comparative example and Example 1 is that the hydrophilic modified ultrafiltration membrane is replaced by a commercially available microporous filter membrane; the commercially available microporous filter membrane is a polypropylene (PP) microporous filter membrane.
[0097] Comparative Example 5: The difference between this comparative example and Example 1 is that the hydrophilic modified ultrafiltration membrane is replaced by a commercially available microporous filter membrane; the commercially available microporous filter membrane is a polytetrafluoroethylene (PTFE) microporous filter membrane.
[0098] Test example: Polishing efficiency and effect test.
[0099] Test subjects: Multi-component brighteners prepared in Examples 1-8 and Comparative Examples 1-5.
[0100] Polishing samples: copper plate, 304 stainless steel.
[0101] Test method: On the same polishing machine, different test objects are used to polish the polished samples (30cm*30cm plates) of the same material. The test objects are used in a unified amount, and the loss and scratch amount of each polished sample are tested within 20 minutes; the loss amount is the thickness of the polished sample surface worn away (lost), which is measured by a three-dimensional profile measuring instrument; the scratch amount is the number of scratches and pits per unit area, which is observed and tested by a wafer appearance detector.
[0102] Test results: See Table 1.
[0103] Table 1. Test data in the test example
[0104]
[0105]
[0106] Result analysis: Analyze Examples 1-8 and combine the data in Table 1 and Figure 1-2 It can be seen that when the brightener prepared by the present invention is used to polish copper plates and 304 stainless steel plates, the loss of the plates within a certain period of time is large, that is, the polishing efficiency is high, and the scratch amount is small, that is, the polishing effect is excellent.
[0107] Analyze Example 1 and Comparative Examples 1-5 and combine the data in Table 1 and Figure 1-2 It can be seen that the present invention has a significant effect on the nano-SiO 2 Modification treatment was performed to obtain modified nano-SiO 2, which is beneficial to improving polishing efficiency and improving polishing effect; the present invention adopts a homemade hydrophilic modified ultrafiltration membrane for impurity removal, which can synergistically improve polishing efficiency and improve polishing effect, and its improvement effect is significantly better than that of ordinary commercially available microporous filter membranes.
[0108] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0109] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A multi-component brightener impurity removal process, characterized in that: The steps include: S1, using 3-aminopropyltriethoxysilane to modify nano-SiO2 to obtain modified nano-SiO2; S2, dispersing 10 parts of the modified nano-SiO2 obtained in S1 in 35-50 parts of deionized water by weight to obtain a dispersed particle liquid; S3, using a hydrophilic modified ultrafiltration membrane to filter the dispersed particle liquid obtained in S2, intercepting the unmodified nano-SiO2, and obtaining a decontaminated particle liquid; S4, centrifugally separating the impurity-removed particle liquid obtained in S3, and vacuum drying to obtain purified modified SiO2; S5, by weight, 1-2 parts of an oxidant, 2-3 parts of a stabilizer, 2-3 parts of a chelating agent, 10-15 parts of a wetting agent, 28-35 parts of deionized water and 30 parts of the purified modified SiO2 obtained in S4 are mixed to obtain a multi-component brightener; The specific preparation steps of the modified nano-SiO2 are as follows: A1. Add 40 g of nano-SiO2 into 1000 mL of toluene and disperse by ultrasonic at room temperature for 30 min to obtain a suspension. A2, adding 18.2 g of 3-aminopropyltriethoxysilane to the suspension obtained in A1, and ultrasonically dispersing at room temperature for 5 min to obtain a dispersion; A3, transfer the dispersion obtained in A2 into a thermostatic bath, and react at 90°C for 6 hours to obtain a reaction solution; A4, at room temperature, centrifuge the reaction solution obtained in A3 and vacuum dry it to obtain modified nano-SiO2; The preparation method of the hydrophilic modified ultrafiltration membrane is as follows: B1. Mix 15-25 parts of polysulfone, 70-80 parts of N,N-dimethylacetamide, 3-5 parts of polyvinyl pyrrolidone and 4-7 parts of acrylamide by weight, and mechanically stir at 60°C for 6-8h to obtain a hydrophilic casting solution; B2, the hydrophilic casting liquid obtained in B1 was allowed to stand for 24 hours at room temperature for degassing, poured onto a glass plate, scraped at a uniform speed with a scraper to form a liquid film of uniform thickness, and then quickly placed in a deionized water coagulation bath, and the hydrophilic modified ultrafiltration membrane was obtained when the film layer completely separated from the glass plate on its own; The oxidant is hydrogen peroxide, the stabilizer is ferrous chloride, the chelating agent includes ethylenediaminetetraacetic acid and / or nitrilotriacetic acid, and the wetting agent includes stearic acid and acetone.
2. The method for removing impurities from a multi-component brightener according to claim 1, characterized in that: The particle size of the nano-SiO2 is 10-40nm.
3. The method for removing impurities from a multi-component brightener according to claim 1, characterized in that: In both A1 and A2, a 300W ultrasonic cleaner was used for ultrasonic dispersion.
4. The method for removing impurities from a multi-component brightener according to claim 1, characterized in that: In both S4 and A4, centrifugal separation was performed at room temperature and 12000r / min.
5. The method for removing impurities from a multi-component brightener according to claim 1, characterized in that: The specific operation steps of S2 are as follows: weigh 10 parts of modified nano-SiO2 and 35-50 parts of deionized water by weight, slowly add the weighed modified nano-SiO2 into the deionized water, stir with a magnetic stirrer at a speed of 500-800rpm and a stirring time of 0.5-2h to obtain a dispersed particle liquid.
6. The method for removing impurities from a multi-component brightener according to claim 1, characterized in that: The mass ratio of stearic acid to acetone in the wetting agent is 2:3-4.
Citation Information
Patent Citations
Polishing agent for renewing polished tiles, stones and artificial stones
CN101838503A
High-efficiency diamond polishing agent and preparation method thereof
CN104059539A
Production of high-purity suspensions containing precipitated silicas by electrodialysis
CN102348493A
Chemical mechanical polishing slurry composition and method for producing semiconductor device using the same
CN102585704A
Preparation method of hydrophilic ultra-filtration membrane
CN102764596A