A nitrogen-carbon-modified perovskite antisilicon catalyst, its preparation method and application
By loading a nitrogen carbide layer onto the surface of the perovskite catalyst to form a heterostructure, the problem of easy deactivation of perovskite catalysts in silicon-containing wastewater was solved, achieving high efficiency, stability and long lifespan of the catalyst, and improving the effect of catalytic ozone oxidation treatment.
Patent Information
- Application Number
- CN202211450601.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-19
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-11-19
AI Technical Summary
Existing perovskite catalysts are prone to deactivation due to silicate deposition when treating silicon-containing wastewater, resulting in shortened lifespan and inability to be recycled, causing resource waste and increased enterprise costs.
The perovskite catalyst modified with nitrogen carbide forms a heterostructure by loading a nitrogen carbide layer on the surface of perovskite particles, thereby improving the catalyst's anti-silicon properties and stability. The preparation method includes co-precipitation, drying, calcination, and physical mixing and roasting of the nitrogen carbide source.
It significantly improved the stability and catalytic performance of the catalyst in silicon-containing wastewater, extended its service life, and demonstrated excellent anti-silicon properties and activity in catalytic ozone oxidation treatment, with a total organic carbon removal rate of over 60% and a m-cresol conversion rate of over 98%.
Smart Images

Figure SMS_21 
Figure SMS_22 
Figure HDA0003951443170000011
Abstract
Description
Technical Field
[0001] This application relates to the field of catalytic ozone oxidation technology, and in particular to a nitrogen carbide-modified perovskite antisilicon catalyst, its preparation method, and its application. Background Technology
[0002] In recent years, with the rapid development of industrialization, globalization, and manufacturing, large amounts of organic chemicals have been discharged into water bodies, causing serious environmental pollution. Advanced oxidation processes (AOP) have proven to be the most effective way to remove recalcitrant organic pollutants from wastewater. Catalytic wet ozone oxidation (CWOO) is a novel method developed in recent years for degrading organic pollutants at ambient temperature and pressure. It overcomes the shortcomings of ozone oxidation alone, greatly improving the utilization rate and oxidation capacity of ozone. The catalytic effect of a catalyst is inseparable from its active components. Commonly used heterogeneous catalysts mainly include: transition metals and their oxides, noble metal oxides, rare earth metal element oxides, and composite oxides.
[0003] Perovskite catalysts are cubic crystal system composite metal oxides. Their spatial structure determines their good stability and catalytic activity, so they are widely used in various fields. At the same time, scholars have also conducted in-depth research on their preparation methods (CN112569968B, CN111036285A, CN106229412B, CN111686755A, CN110026185A).
[0004] In the field of catalysis, the presence of silicon in actual coal chemical wastewater is unavoidable. Silicates deposit on the catalyst surface, causing poisoning and deactivation that is irreversible. This significantly shortens the catalyst's lifespan, and the silicon-coated catalyst cannot be recycled, requiring treatment as hazardous waste, resulting in substantial waste and increased operating costs for enterprises. Researchers typically use material modification methods to modulate various properties of the catalyst.
[0005] In recent years, a metal-free nitrogen carbide material has received widespread attention due to its numerous advantages, such as simple preparation method, low cost, and good stability (CN107029774B, CN105731397A, CN102931418B, CN105126893A). This has laid a good foundation for the use of nitrogen carbide to modify perovskite materials. Summary of the Invention
[0006] In view of this, the purpose of this application is to provide a nitrogen carbide-modified perovskite material, its preparation method and application, which can maintain excellent degradation effect on organic pollutants in silicon-containing wastewater.
[0007] According to one aspect of this application, a nitrogen carbide-modified perovskite anti-silicon catalyst is provided, the nitrogen carbide-modified perovskite anti-silicon catalyst comprising a nitrogen carbide layer and perovskite particles supported on the surface of the nitrogen carbide layer; In the nitrogen carbide-modified perovskite antisilicon catalyst, the mass content of nitrogen carbide is 10~90 wt%; Optionally, in the nitrogen carbide-modified perovskite antisilicon catalyst, the mass content of nitrogen carbide is any value or a range between 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, and 90 wt%.
[0008] The perovskite particles loaded on the surface of the nitrogen carbide layer have a particle size of 30~80nm; Optionally, the perovskite particles loaded on the surface of the nitrogen carbide layer have a particle size of any value among 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, and 80 nm, or a range between any two.
[0009] The thickness of the nitride layer is 10~100 nm; Optionally, the thickness of the nitrogen carbide layer is any value or a range between 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, and 100 nm.
[0010] The pore size of the nitrogen carbide-modified perovskite antisilicon catalyst is 8.9~14.9 nm; Optionally, the pore size of the nitrogen carbide-modified perovskite antisilicon catalyst is any value or a range between 8.9 nm, 9 nm, 9.5 nm, 10 nm, 10.5 nm, 11 nm, 11.5 nm, 12 nm, 12.5 nm, 13 nm, 13.5 nm, 14 nm, 14.5 nm, and 14.9 nm.
[0011] The specific surface area of the nitrogen carbide-modified perovskite antisilicon catalyst is 9~31 m². 2 / g.
[0012] Optionally, the specific surface area of the nitrogen carbide-modified perovskite antisilicon catalyst is 9 m². 2 / g、10 m 2 / g, 15m 2 / g、20 m 2 / g、25 m 2 / g、30 m 2 / g、31 m2 Any value in / g or any range between the two.
[0013] The perovskite is of type AB perovskite; The A-site element of the perovskite is selected from at least one of La, Ca, and Sr; The B-site element of the perovskite is selected from at least one of Fe, Co, Ni, Mn, and Cu.
[0014] The lattice spacing of the perovskite particles loaded on the surface of the nitrogen carbide layer is 0.25~0.27 nm; Optionally, the lattice spacing of the perovskite particles loaded on the surface of the nitrogen carbide layer is any value among 0.25 nm, 0.26 nm, and 0.27 nm, or any value between any two.
[0015] The exposed crystal planes of the nitride layer are (100) and (022).
[0016] The nitrogen carbide has a layered structure; The perovskite forms a heterostructure with layered nitrogen carbides.
[0017] The catalyst has a type IV isotherm and exhibits mesoporous or mesoporous properties.
[0018] The nitrogen-modified perovskite antisilicon catalyst is more likely to have a positive charge on its surface compared to the unmodified catalyst. The surface of the nitrogen-modified perovskite antisilicon catalyst is positively charged in the pH range of 3 to 10.
[0019] According to another aspect of this application, a method for preparing a nitrogen carbide-modified perovskite antisilicon catalyst is provided, comprising the following steps: (1) Mix an aqueous solution containing precursor A and precursor B with an aqueous solution containing a precipitant, precipitate, age, dry, and calcine to obtain the perovskite; (2) The perovskite obtained in (1) is physically mixed with a nitrogen carbide source, dried and calcined to obtain the nitrogen carbide-modified perovskite anti-silicon catalyst; A is selected from at least one of La, Ca, and Sr; The B is selected from at least one of Fe, Co, Ni, Mn, and Cu.
[0020] The A precursor is selected from at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of La; at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of Ca; and at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of Sr. The B precursor is selected from at least one of the following: Fe nitrate, sulfate, acetate, phosphate, and chloride; Co nitrate, sulfate, acetate, phosphate, and chloride; Ni nitrate, sulfate, acetate, phosphate, and chloride; Mn nitrate, sulfate, acetate, phosphate, and chloride; and Cu nitrate, sulfate, acetate, phosphate, and chloride. In the aqueous solution containing precursor A and precursor B, the concentration of precursor A is 2-4 wt%, calculated as the mass fraction of lanthanum, a metal element in precursor A. Optionally, in the aqueous solution containing precursor A and precursor B, the concentration of precursor A is any value from 2 wt%, 2.5 wt%, 2.9 wt%, 3 wt%, 3.5 wt%, 4 wt%, or any range between both.
[0021] In the aqueous solution containing precursor A and precursor B, the concentration of precursor B is 0~1.2wt%, calculated as the mass fraction of iron, a metallic element in precursor B. Optionally, in the aqueous solution containing precursor A and precursor B, the concentration of precursor B is any value among 0 wt%, 0.5 wt%, 1 wt%, and 1.2 wt%, or any range between both.
[0022] The volume ratio of the aqueous solution containing precursor A and precursor B to the aqueous solution containing the precipitant is 1:4 to 4:1. Optionally, the volume ratio of the aqueous solution containing precursor A and precursor B to the aqueous solution containing the precipitant is any value from 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, or any range between the two.
[0023] The precipitant is selected from at least one of PEG1000, PEG2000, PEG4000, PEG6000, PEG10000, and PEG20000; In the aqueous solution containing the precipitant, the concentration of the precipitant is 0.1~1wt%; Optionally, in the aqueous solution containing the precipitant, the concentration of the precipitant is any value among 0.1 wt%, 0.5 wt%, and 1 wt%, or a range between any two.
[0024] The mixing process controls the pH to be between 8 and 12. Optionally, the mixing process controls the pH to any value among 8, 9, 10, 11, and 12, or a range between any two.
[0025] The precipitation temperature is 10~45℃; Optionally, the precipitation temperature is any value among 10℃, 15℃, 20℃, 25℃, 30℃, 35℃, 40℃, and 45℃, or a range between any two.
[0026] The precipitation time is 1-4 hours; Optionally, the precipitation time is any value among 1h, 2h, 3h, and 4h, or a range between any two.
[0027] The aging temperature is 70~100℃; Optionally, the aging temperature is any value among 70°C, 80°C, 90°C, and 100°C, or a range between any two.
[0028] The aging time is 12~48 hours; Optionally, the aging time is any value among 12h, 18h, 24h, 30h, 36h, 42h, and 48h, or a range between any two.
[0029] The drying temperature is 120~160℃; Optionally, the drying temperature is any value among 120°C, 130°C, 140°C, 150°C, and 160°C, or a range between any two.
[0030] The drying time is 12-48 hours; Optionally, the drying time is any value among 12h, 18h, 24h, 30h, 36h, 42h, and 48h, or a range between any two.
[0031] The calcination temperature is 600~1000℃; Optionally, the calcination temperature is any value among 600℃, 700℃, 800℃, 900℃, and 1000℃, or a range between any two.
[0032] The calcination time is 2 to 12 hours.
[0033] Optionally, the calcination time is any value among 2h, 4h, 6h, 8h, 10h, and 12h, or a range between any two.
[0034] The nitrogen carbide source is selected from at least one of melamine, dicyandiamide, and urea; The mass ratio of the perovskite obtained in (1) to the nitrogen carbide source is 9:1 to 1:9; Optionally, the mass ratio of the perovskite obtained in (1) to the nitrogen carbide source is any value among 9:1, 4:1, 2:1, 1:1, 1:2, 1:4, 1:9 or any range between the two.
[0035] The physical mixing includes grinding and stirring with water; The grinding time is 2-10 minutes; Optionally, the grinding time is any value among 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, and 10 min, or a range between any two.
[0036] During the water addition and stirring process, the mass of water added is 2 to 20 times that of the nitrogen carbide source; Optionally, during the water addition and stirring process, the mass of water added is any value among 2, 5, 10, 15, and 20 times the mass of the nitrogen carbide source, or any value within a range of both.
[0037] The stirring time for adding water is 2 to 12 hours.
[0038] Optionally, the stirring time for adding water and stirring is any value among 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, and 12h, or a range between any two.
[0039] The stirring speed for adding water is 200~2000 r / min.
[0040] Optionally, the stirring speed for adding water is any value among 200 r / min, 500 r / min, 1000 r / min, 1500 r / min, and 2000 r / min, or a range between any two.
[0041] The drying temperature is 50~100℃; Optionally, the drying temperature is any value among 50°C, 60°C, 70°C, 80°C, 90°C, and 100°C, or a range between any two.
[0042] The drying time is 10~48 hours; Optionally, the drying time is any value among 10h, 12h, 18h, 24h, 30h, 36h, 42h, and 48h, or a range between any two.
[0043] The roasting temperature is 300~600℃; Optionally, the calcination temperature is any value among 300°C, 400°C, 500°C, and 600°C, or a range between any two.
[0044] The heating rate for calcination is 5~20℃ / min; Optionally, the heating rate of the calcination is any value among 5℃ / min, 10℃ / min, 15℃ / min, and 20℃ / min, or a range between any two.
[0045] The roasting time is 2-8 hours; Optionally, the roasting time is any value among 2h, 3h, 4h, 5h, 6h, 7h, and 8h, or a range between any two.
[0046] The calcination atmosphere is a non-reactive gas atmosphere; The inactive gas atmosphere is selected from at least one of nitrogen, helium, and argon.
[0047] The flow rate of the inactive gas atmosphere is 200~1000 mL / min.
[0048] Optionally, the flow rate of the inactive gas atmosphere is any value or a range between 200 mL / min, 300 mL / min, 400 mL / min, 500 mL / min, 600 mL / min, 700 mL / min, 800 mL / min, 900 mL / min, and 1000 mL / min.
[0049] Before calcination, the dried material is sealed by placing it in a crucible. If the crucible is completely open, the degree of openness is defined as 100%; if the crucible is completely closed, the degree of openness is defined as 0%. The degree of openness during calcination is 0-30%.
[0050] Optionally, the openness is selected from any value of 0%, 5%, 10%, 20%, 30%, or a range between any two.
[0051] The synthesized catalyst has surface hydroxyl groups and good oxygen vacancy characteristics. Oxygen vacancies can serve as active sites for the catalyst, capturing ozone and converting it into reactive oxygen free radicals. The variable valence state of the metal active component can promote electron cycling. The excellent conductivity of nitrogen carbide helps to accelerate the electron transport rate in the catalytic reaction process, thus speeding up the reaction. At the same time, it also promotes the anti-silicon properties and stability of the catalyst.
[0052] The modification with nitrogen carbide greatly improves the anti-silicon properties and stability. The nitrogen carbide-modified perovskite material of this application is used as a catalyst for the first time in the catalytic ozone oxidation treatment of silicon-containing wastewater. The catalyst can maintain excellent stability and catalytic performance in silicon-containing wastewater.
[0053] According to another aspect of this application, a method for treating silicon-containing organic wastewater by catalytic ozone oxidation is provided, comprising the following steps: Silicon-containing organic wastewater is contacted with a catalyst and treated in an ozone-containing atmosphere. The catalyst is selected from the nitrogen-modified perovskite anti-silicon catalyst described above or the nitrogen-modified perovskite anti-silicon catalyst prepared by the above preparation method.
[0054] The silicon-containing organic wastewater contains at least one of monosilicic acid, disilicic acid, and polysilicic acid. The silicon content in the silicon-containing organic wastewater is 10~500 mg / L; based on the mass of silicon dioxide; Optionally, the silicon content in the silicon-containing organic wastewater is any value or a range between 10 mg / L, 50 mg / L, 100 mg / L, 200 mg / L, 300 mg / L, 400 mg / L, and 500 mg / L.
[0055] Optionally, the silicon-containing organic wastewater may also contain at least one of m-cresol, o-cresol, p-cresol, maleic acid, acetic acid, bisphenol A, bisphenol F, and acrylic acid.
[0056] The reaction temperature is 10~30℃; Optionally, the temperature of the reaction is any value among 10°C, 20°C, and 30°C, or a range between any two.
[0057] The reaction time is 10-120 min; Optionally, the reaction time is any value or a range between 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, and 120 min.
[0058] In the ozone-containing atmosphere, the ozone concentration is 0~200 mg / L; Optionally, in the ozone-containing atmosphere, the ozone concentration is any value among 0 mg / L, 50 mg / L, 100 mg / L, 150 mg / L, and 200 mg / L, or a range between any two.
[0059] In the ozone-containing atmosphere, the ozone flow rate is 0~80 ml / min; Optionally, in the ozone-containing atmosphere, the ozone flow rate is any value among 0 ml / min, 20 ml / min, 40 ml / min, 60 ml / min, and 80 ml / min, or a range between any two.
[0060] The mass ratio of the catalyst to the solid-liquid mixture of the silicon-containing organic wastewater is 0.5~5 g / L; Optionally, the mass of the catalyst and the solid-liquid ratio of the silicon-containing organic wastewater are any value from 0.5 g / L, 1 g / L, 2 g / L, 3 g / L, 4 g / L, 5 g / L, or any range between two.
[0061] The pH is controlled at 3-11 during the treatment process.
[0062] Optionally, the pH is controlled during the treatment process to be any value among 3, 4, 5, 6, 7, 8, 9, 10, and 11, or a range between any two.
[0063] Optionally, the silicon-containing wastewater also includes Ca. 2+ Mg 2+ One or more types of plasma.
[0064] Optionally, the Ca 2+ Mg 2+ The plasma concentration is 10~2000 mg / L.
[0065] Optionally, the Ca 2+ Mg 2+ The plasma concentration is any value among 10 mg / L, 50 mg / L, 100 mg / L, 500 mg / L, 1000 mg / L, 1500 mg / L, 2000 mg / L, or any range between two of them.
[0066] Optionally, the reaction uses a batch reactor used in batch ozone oxidation / catalytic ozone oxidation experiments; the reactor is horn-shaped and has an ozone inlet and an outlet. The reactor has a volume of 250 mL.
[0067] The ozone is reacted in an ozone generator (CF-G-3-10g, Qingdao Guolin Environmental Protection Technology Co., Ltd.) to produce high-purity oxygen (99.999%). The ozone is dispersed through the aeration head at the air inlet and then enters the reaction liquid.
[0068] The reaction solution contains a silicon source and pollutants.
[0069] The ozone flow rate, ozone concentration, reaction time, catalyst dosage, and reaction pH were set according to the experimental conditions.
[0070] Optionally, during the reaction process, a rotor is added to the reactor for continuous stirring, and the stirring speed is 500~2000 r / min.
[0071] Samples were periodically taken from the reactor to analyze the conversion rate of relevant substances, the removal rate of total organic carbon, and the anti-silicon properties of the catalyst.
[0072] The silicon content in the solution was determined using the silicomolybdenum blue spectrophotometric method, with a detection range of 0–4 mg / L. The determination steps are as follows: (1) Accurately transfer a certain amount of silica standard working solution and add silica-free water to 5~10mL; (2) Add 0.15~0.3mL of ammonium molybdate sulfate solution, shake well, and let stand for 10min; (3) Add 0.15~0.3mL of 10% oxalic acid solution, shake well, and let stand for 5min; (4) Add 0.15~0.3mL of ferrous ammonium sulfate solution, mix well, and let stand for 15min; (5) The absorbance of the above solution was measured at 815 nm, and a blank reference test was performed at the same time.
[0073] A magnetic stirrer was turned on, and a rotor was added to the reactor to continuously stir the mixture at a speed of 1000 rpm. The reaction temperature was 20°C. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicon properties of the catalyst. The organic matter degradation performance of the samples was determined using a Shimadzu total organic carbon analyzer. The m-cresol conversion rate was determined using HPLC. The silicon concentration was determined using a spectrophotometer.
[0074] m-Cresol Conversion Rate =
[0075] Where C0 is the initial m-cresol concentration, C t Let t be the concentration of cresol at time t.
[0076] Total organic carbon removal rate =
[0077] Wherein, TOC0 is the initial total organic carbon, and TOC t Let t be the total organic carbon at time t.
[0078] Silicon resistance = /
[0079] in, It refers to the amount of silicon absorbed by the catalyst. It refers to the quality of the catalyst; the smaller the W value, the stronger the catalyst's resistance to silicon.
[0080] The silicon content in the solution was determined using the molybdenum blue spectrophotometric method. Accurately transfer a certain amount of silica standard working solution, add silica-free water to 5-10 mL; add 0.15-0.3 mL of ammonium molybdate sulfate solution, shake well, and let stand for 10 min; add 0.15-0.3 mL of 10% oxalic acid solution, shake well, and let stand for 5 min; then add 0.15-0.3 mL of ferrous ammonium sulfate solution, mix well, and let stand for 15 min; measure its absorbance at 815 nm, and perform a blank reference test at the same time.
[0081] The beneficial effects of this application include: 1) The perovskite antisilicon catalyst modified with nitrogen carbide provided in this application can significantly inhibit the influence of wastewater on the catalyst, enhance the catalyst stability, avoid catalyst deactivation, and extend the catalyst service life. The treatment of the openness before calcination during the preparation process plays a very important role in the material.
[0082] 2) The nitrogen carbide-modified perovskite anti-silicon catalyst provided in this application has a heterostructure formed by the combination of perovskite and layered nitrogen carbide. The catalyst with the heterostructure has a significantly improved anti-silicon performance in the catalytic ozone oxidation treatment of silicon-containing wastewater, exhibiting excellent activity and stability.
[0083] 3) The nitrogen-modified perovskite anti-silicon catalyst provided in this application exhibits a higher likelihood of positive charge on its surface compared to unmodified materials. The surface of the nitrogen-modified perovskite material is positively charged within a pH range of 3-10. It possesses surface hydroxyl groups and excellent oxygen vacancy characteristics. Oxygen vacancies can serve as active sites for the catalyst, capturing ozone and converting it into reactive oxygen free radicals. The variable valence state of the metal active component promotes electron cycling, and the excellent conductivity of nitrogen-modified materials helps accelerate electron transport during the catalytic reaction, thus speeding up the reaction. Simultaneously, it promotes the anti-silicon properties and stability of the catalyst. Nitrogen-modified materials significantly enhance anti-silicon properties and stability. For the first time, nitrogen-modified perovskite materials are used as catalysts for the catalytic ozone oxidation treatment of silicon-containing wastewater, maintaining excellent stability and catalytic performance in silicon-containing wastewater.
[0084] (4) The carbonyl modified perovskite antisilicon catalyst provided in this application improves the antisilicon performance by more than 3 times in the catalytic ozone oxidation treatment of silicon-containing organic wastewater, with a total organic carbon removal rate of more than 60% and a m-cresol conversion rate of more than 98%. Attached Figure Description
[0085] Figure 1In the figures, (a) is a comparison chart of the TOC removal rates of the perovskite catalyst modified with nitrogen carbide in Example 1 of this application, compared with that of perovskite alone in Comparative Example 1 and nitrogen carbide alone in Comparative Example 2, and ozone alone; (b) is a comparison chart of the reaction rate constants of the perovskite catalyst modified with nitrogen carbide in Example 1 of this application, compared with that of perovskite alone in Comparative Example 1 and nitrogen carbide alone in Comparative Example 2, and ozone alone.
[0086] Figure 2 This is a transmission electron microscope (TEM) image of the nitrogen carbide-modified perovskite catalyst of Example 1 of this application.
[0087] Figure 3 This is a scanning electron microscope image of the nitrogen carbide-modified perovskite catalyst of Example 1 of this application.
[0088] Figure 4 This is a Zeta potential test diagram comparing the nitrogen carbide-modified perovskite catalyst of Example 1 of this application with the single perovskite catalyst of Comparative Example 1.
[0089] Figure 5 The XRD patterns are comparison images of the perovskite catalysts modified with nitrogen carbide in Examples 1-3 of this application with those of Comparative Example 1 (perovskite alone) and Comparative Example 2 (nitrogen carbide alone).
[0090] Figure 6 The figures show nitrogen adsorption-desorption test results of the perovskite catalysts modified with nitrogen carbide in Examples 1-3 of this application, compared with perovskite alone in Comparative Example 1 and nitrogen carbide alone in Comparative Example 2. Detailed Implementation
[0091] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0092] The technical solution of this application is described in detail below with reference to the embodiments, but this application is not limited to these specific embodiments.
[0093] X-ray diffraction (XRD), with a scanning angle range of 10°. -90 ,PANalytical, X'Pert PRO.
[0094] Scanning electron microscopy (SEM) was performed using a Hitach S-4800 high-resolution field emission scanning electron microscope (SEM) manufactured by Hitach Corporation of Japan to observe the surface morphology and structural features of the samples. Before the SEM characterization tests, the samples were ground to a particle size of 200 mesh, and then a small amount of sample was attached to the surface of a copper disk for measurement. To ensure good conductivity, the samples were vacuum-sputtered with gold before the tests.
[0095] The N2 physical adsorption-desorption (BET) test was performed using a NOVA4000e physical adsorption instrument manufactured by Quanta Instruments, USA, to detect the specific surface area and pore size distribution of the samples. Detection conditions: N2 as the adsorbed gas, He as the carrier gas, catalyst dosage of 0.1~0.2 g, 90℃ for half an hour, 300℃ for three hours. The BET specific surface area was calculated using the BJH method, and the micropore specific surface area was calculated using the T-chart method.
[0096] High-resolution transmission electron microscopy (HRTEM) was performed using a JEOL-manufactured JEM-2100 high-resolution transmission electron microscope at an accelerating voltage of 120 kV.
[0097] Zeta potential was measured using the Nano-ZS ZEN3600 nanoparticle size and zeta potential analyzer.
[0098] The performance of the samples in degrading organic matter was determined using a Shimadzu total organic carbon analyzer.
[0099] The conversion rate of m-cresol was determined by HPLC high-performance liquid chromatography.
[0100] The silicon concentration was determined using a spectrophotometer.
[0101] m-Cresol Conversion Rate =
[0102] Where C0 is the initial m-cresol concentration, C t Let t be the concentration of cresol at time t.
[0103] Total organic carbon removal rate =
[0104] Wherein, TOC0 is the initial total organic carbon, and TOC t Let t be the total organic carbon at time t.
[0105] Silicon resistance = /
[0106] in, It refers to the amount of silicon absorbed by the catalyst. It refers to the quality of the catalyst; the smaller the W value, the stronger the catalyst's resistance to silicon.
[0107] The silicon content in the solution was determined using the molybdenum blue spectrophotometric method. Accurately transfer a certain amount of silica standard working solution, add silica-free water to 5-10 mL; add 0.15-0.3 mL of ammonium molybdate sulfate solution, shake well, and let stand for 10 min; add 0.15-0.3 mL of 10% oxalic acid solution, shake well, and let stand for 5 min; then add 0.15-0.3 mL of ferrous ammonium sulfate solution, mix well, and let stand for 15 min; measure its absorbance at 815 nm, and perform a blank reference test at the same time.
[0108] To further illustrate this application, the following detailed description, in conjunction with embodiments, of a nitrogen carbide-modified perovskite antisilicon catalyst, its preparation method, and its application, is provided in this application. However, these descriptions should not be construed as limiting the scope of protection of this application.
[0109] Comparative Example 1 For ease of comparison with the product of this application, unmodified perovskite is provided as Comparative Example 1.
[0110] (a) Coprecipitation titration: 18g La(NO3)3·6H2O, 4g Fe(NO3)3·9H2O, and 11g Mn(NO3)2 (50%) were dissolved in 100 mL of deionized water as precursors. 5 mL of ammonia was dissolved in 92 mL of deionized water, and 0.05g of PEG was added as a precipitant. The nitrate precursor was added to the precipitant with stirring and mixed thoroughly.
[0111] (ii) Aging process: After aging at 100 ºC for 48 hours, it is repeatedly washed with deionized water until neutral.
[0112] (iii) Drying process: Dry in an oven at 120 ºC for 12 hours.
[0113] (iv) Calcination of the catalyst: calcination at 800ºC for 6 hours.
[0114] The LaFeMnO3 catalyst is thus obtained, which is Comparative Example 1#, and can be referred to as LFMO catalyst below.
[0115] Comparative Example 2 For ease of comparison with the product of this application, nitrogen carbide is provided separately as comparative example 2.
[0116] Place 20g of dicyandiamide in a crucible and seal it. Adjust the opening degree to 5%. Heat the crucible to 400℃ at a rate of 10℃ / min and calcine for 5 hours. The nitrogen flow rate is 500mL / min until the calcine process is completed. After the temperature inside the furnace drops, turn off the nitrogen gas to obtain the desired nitrogen carbide material (g-C3N4), which is comparative example 2# and can be referred to as CN below.
[0117] Example 1 (a) Synthesis of perovskite catalyst by coprecipitation method, the preparation process is the same as Comparative Example 1.
[0118] (ii) Physical mixing of perovskite and nitrogen carbide source: 20g of perovskite and 5g of dicyandiamide were mixed and ground in a mortar for 2min. Then 50mL of deionized water was added and stirred at 800r / min for 5h. After stirring, the mixture was placed in an oven and dried at 70℃ for 40h.
[0119] (III) Calcination process: The dried sample is placed in a crucible and sealed. The opening degree is adjusted to 5%. The temperature is increased to 400℃ at a rate of 10℃ / min. The calcination time is 5h and the nitrogen flow rate is 500mL / min until the calcination process is completed. After the temperature in the furnace is cooled down, the nitrogen gas is turned off to obtain the required nitrogen carbide modified perovskite material, which is sample 1#, and can be referred to as LFMO-CN-1 below.
[0120] The prepared nitrogen carbide-modified perovskite catalyst has a perovskite particle size of 30-80 nm and a lattice spacing of 0.25-0.27 nm; a layered nitrogen carbide thickness of 10-100 nm and exposed crystal faces of (100) and (022); the material has a type IV isotherm, mesoporous or mesoporous properties, and a specific surface area of 31 m². 2 / g, with a pore size of 11.9nm; the surface of the perovskite material modified with nitrogen carbide is positively charged in the pH range of 3~10; and the surface contains a large number of oxygen vacancies and hydroxyl groups.
[0121] Intermittent catalytic ozone oxidation experiments were conducted using an intermittent reactor with a volume of 250 mL. Ozone was reacted with an ozone generator (CF-G-3-10g, Qingdao Guolin Environmental Protection Technology Co., Ltd.) to generate high-purity oxygen (99.999%). Rubber hoses were used to connect the inlet and outlet of the gas.
[0122] A solution containing 100 mg / L m-cresol and 80 mg / L silica was prepared, and the pH was adjusted to 8.0. 2 g / L of the aforementioned nitrogen carbide-modified perovskite anti-silicon catalyst was then added to initiate the reaction. The ozone flow rate was set to 60 mL / min, the ozone concentration to 130 mg / L, and the reaction time to 60 min, according to the experimental conditions. The ozone was dispersed through the aeration head at the inlet and then introduced into the reaction solution.
[0123] During the reaction, a rotor was continuously stirred in the reactor at a speed of 1000 r / min. The reaction temperature was 20℃. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicon performance of the catalyst. The results are shown in Table 1. The performance of the samples in degrading organic matter was determined using a Shimadzu total organic carbon analyzer. The conversion rate of m-cresol was determined using HPLC. The silicon concentration was determined using a spectrophotometer.
[0124] m-Cresol Conversion Rate =
[0125] Where C0 is the initial m-cresol concentration, C t Let t be the concentration of cresol at time t.
[0126] Total organic carbon removal rate =
[0127] Wherein, TOC0 is the initial total organic carbon, and TOC t Let t be the total organic carbon at time t.
[0128] Silicon resistance = /
[0129] in, It refers to the amount of silicon absorbed by the catalyst. It refers to the quality of the catalyst; the smaller the W value, the stronger the catalyst's resistance to silicon.
[0130] The silicon content in the solution was determined using the molybdenum blue spectrophotometric method. Accurately transfer a certain amount of silica standard working solution and add silica-free water to 5 mL; add 0.15 mL of ammonium molybdate sulfate solution, shake well, and let stand for 10 min; add 0.15 mL of 10% oxalic acid solution, shake well, and let stand for 5 min; then add 0.15 mL of ferrous ammonium sulfate solution, mix well, and let stand for 15 min; measure its absorbance at 815 nm, and perform a blank reference test at the same time.
[0131] Using sample 1# as a typical representative and a comparative example, the test results are shown in the figure below. Figure 1 As shown in the figure, sample 1# exhibited superior treatment performance during the reaction process, achieving the highest TOC removal rate. Figure 1 As shown in (a), the reaction rate constant is as follows: Figure 1 As shown in (b), it is significantly superior to the perovskite, nitrogen carbide and ozone oxidation alone in the comparative examples.
[0132] Example 2 (a) Synthesis of perovskite catalyst by coprecipitation method, the preparation process is the same as Comparative Example 1.
[0133] (ii) Physical mixing of perovskite and nitrogen carbide source: 10g of perovskite and 10g of dicyandiamide are mixed and ground in a mortar for 2min. Then 50mL of deionized water is added and stirred at 800r / min for 5h. After stirring, the mixture is placed in an oven and dried at 70℃ for 40h.
[0134] (III) Calcination process: The dried sample is placed in a crucible and sealed. The opening degree is adjusted to 5%. The temperature is increased to 400℃ at a rate of 10℃ / min. The calcination time is 5h and the nitrogen flow rate is 500mL / min until the calcination process is completed. After the temperature in the furnace is cooled down, the nitrogen gas is turned off to obtain the required nitrogen carbide modified perovskite material, which is sample 2#, and can be referred to as LFMO-CN-2 below.
[0135] The prepared nitrogen carbide-modified perovskite catalyst has a perovskite particle size of 30-80 nm and a lattice spacing of 0.25-0.27 nm; a layered nitrogen carbide thickness of 10-100 nm and exposed crystal faces of (100) and (022); the material has a type IV isotherm, mesoporous or mesoporous properties, and a specific surface area of 22 m². 2 / g, with a pore size of 12.1nm; the surface of the nitrogen-modified perovskite material is positively charged in the pH range of 3~10.
[0136] The reaction conditions were the same as in Example 1. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicone performance of the catalyst. The results are shown in Table 1.
[0137] Example 3 (a) Synthesis of perovskite catalyst by coprecipitation method, the preparation process is the same as Comparative Example 1.
[0138] (ii) Physical mixing of perovskite and nitrogen carbide source: 5g of perovskite and 20g of dicyandiamide were mixed and ground in a mortar for 2min. Then 50mL of deionized water was added and stirred at 800r / min for 5h. After stirring, the mixture was placed in an oven and dried at 70℃ for 40h.
[0139] (III) Calcination process: The dried sample is placed in a crucible and sealed. The opening degree is adjusted to 5%. The temperature is increased to 400℃ at a rate of 10℃ / min. The calcination time is 5h and the nitrogen flow rate is 500mL / min until the calcination process is completed. After the temperature in the furnace is cooled down, the nitrogen gas is turned off to obtain the required nitrogen carbide modified perovskite material, which is sample 3#, and can be referred to as LFMO-CN-3 below.
[0140] The prepared nitrogen carbide-modified perovskite catalyst has a perovskite particle size of 30-80 nm and a lattice spacing of 0.25-0.27 nm; a layered nitrogen carbide thickness of 10-100 nm and exposed crystal faces of (100) and (022); the material has a type IV isotherm, mesoporous or mesoporous properties, and a specific surface area of 13 m². 2 / g, with a pore size of 14.9nm; the surface of the nitrogen-modified perovskite material is positively charged in the pH range of 3~11.
[0141] The reaction conditions were the same as in Example 1. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicone performance of the catalyst. The results are shown in Table 1.
[0142] Example 4 (a) Synthesis of perovskite catalyst by coprecipitation method, the preparation process is the same as Comparative Example 1.
[0143] (ii) Physical mixing of perovskite and nitrogen carbide source: 10g of perovskite and 10g of dicyandiamide are mixed and ground in a mortar for 2min. Then 50mL of deionized water is added and stirred at 800r / min for 5h. After stirring, the mixture is placed in an oven and dried at 70℃ for 40h.
[0144] (III) Calcination process: The dried sample is placed in a crucible and sealed. The opening degree is adjusted to 0%. The temperature is increased to 500℃ at a rate of 10℃ / min. The calcination time is 4h and the nitrogen flow rate is 500mL / min until the calcination process is completed. After the temperature in the furnace is cooled down, the nitrogen gas is turned off to obtain the required nitrogen carbide modified perovskite material, which is sample 4#.
[0145] The reaction conditions were the same as in Example 1. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicone performance of the catalyst. The results are shown in Table 1.
[0146] Example 5 (a) Synthesis of perovskite catalyst by coprecipitation method, the preparation process is the same as Comparative Example 1.
[0147] (ii) Physical mixing of perovskite and nitrogen carbide source: 10g of perovskite and 10g of dicyandiamide are mixed and ground in a mortar for 2min. Then 50mL of deionized water is added and stirred at 800r / min for 5h. After stirring, the mixture is placed in an oven and dried at 70℃ for 40h.
[0148] (III) Calcination process: The dried sample is placed in a crucible and sealed. The opening degree is adjusted to 10%. The temperature is increased to 600℃ at a rate of 10℃ / min. The calcination time is 3h and the nitrogen flow rate is 500mL / min until the calcination process is completed. After the temperature in the furnace is cooled down, the nitrogen gas is turned off to obtain the required nitrogen carbide modified perovskite material, which is sample 5#.
[0149] The reaction conditions were the same as in Example 1. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the antisilicic properties of the catalyst, where TOCO = 76.55 mg / L. The results are shown in Table 1.
[0150] Table 1. Comparison of catalytic ozone oxidation and anti-silicon properties of LFMO-CN catalysts
[0151] Table 1 shows that without the addition of a catalyst, the conversion rate of m-cresol was 97.25%, but the TOC removal rate of the wastewater was only 29.85%, indicating poor TOC removal. This means that organic pollutants in the water could not be completely removed, and m-cresol was only converted into an intermediate product. When comparative catalyst 1 was added, both the m-cresol conversion rate and TOC removal rate improved, but the silica resistance was very poor at 3.62. A large value indicates strong silica adsorption capacity and poor silica resistance, which is detrimental to the long-term stability of the catalyst. While comparative catalyst 2 showed relatively excellent silica resistance, the TOC removal rate was almost no better than that of ozone oxidation alone. The poor TOC removal rate hindered the application of comparative catalyst 2 (a nitrogen carbide catalyst alone). However, after combining perovskite with nitrogen carbide to form a nitrogen carbide-modified perovskite catalyst, samples 1#~5# showed ideal results. From the reaction results, the optimized nitrogen carbide-modified perovskite catalyst (LFMO-CN) showed a m-cresol conversion rate of over 99% and a TOC removal rate of over 60%, while also exhibiting excellent anti-silicon properties. Sample 1# catalyst achieved a TOC removal rate of 69.38%, indicating a higher capacity for degrading pollutants in water. Its anti-silicon performance value of 0.85, a relatively low value, suggests excellent anti-silicon properties, which helps maintain high activity over long-term reactions. Comparing samples 1# to 3#, it can be seen that the anti-silicon performance of the modified catalyst increases with the addition of nitrogen carbide; however, excessive nitrogen carbide (3#) leads to a decrease in catalytic effect. Therefore, Example 1, with its excellent degradation effect and anti-silicon properties, is selected as the optimal catalyst.
[0152] Example 6 The catalytic reaction conditions were optimized using the catalyst prepared in Example 1.
[0153] Intermittent catalytic ozone oxidation experiments were conducted using an intermittent reactor with a volume of 250 mL. Ozone was reacted with an ozone generator (CF-G-3-10g, Qingdao Guolin Environmental Protection Technology Co., Ltd.) to generate high-purity oxygen (99.999%). Rubber hoses were used to connect the inlet and outlet of the gas.
[0154] A solution containing 100 mg / L m-cresol and 80 mg / L silica was prepared, and the pH was adjusted to 8.0. 2 g / L of the aforementioned anti-silica catalyst was then added to initiate the reaction. The ozone flow rate was set to 50 mL / min, the ozone concentration to 130 mg / L, and the reaction time to 60 min, according to the experimental conditions. The ozone was dispersed through the aeration head at the inlet and then introduced into the reaction solution.
[0155] During the reaction, a rotor was continuously stirred in the reactor at a speed of 1000 r / min. The reaction temperature was 20℃. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicon performance of the catalyst. The results are shown in Table 2. The organic matter degradation performance of the samples was determined using a Shimadzu total organic carbon analyzer. The m-cresol conversion rate was determined using HPLC. The silicon concentration was determined using a spectrophotometer.
[0156] Example 7 The catalytic reaction conditions were optimized using the catalyst prepared in Example 1.
[0157] Intermittent catalytic ozone oxidation experiments were conducted using an intermittent reactor with a volume of 250 mL. Ozone was reacted with an ozone generator (CF-G-3-10g, Qingdao Guolin Environmental Protection Technology Co., Ltd.) to generate high-purity oxygen (99.999%). Rubber hoses were used to connect the inlet and outlet of the gas.
[0158] A solution of 100 mg / L m-cresol and 10 mg / L silica was prepared, and the pH was adjusted to 8.0. 2 g / L of the aforementioned anti-silica catalyst was then added to initiate the reaction. The ozone flow rate was set to 50 mL / min, the ozone concentration to 130 mg / L, and the reaction time to 60 min, according to the experimental conditions. The ozone was dispersed through the aeration head at the inlet and then introduced into the reaction solution.
[0159] During the reaction, a rotor was continuously stirred in the reactor at a speed of 1000 r / min. The reaction temperature was 20℃. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicon performance of the catalyst. The results are shown in Table 2. The organic matter degradation performance of the samples was determined using a Shimadzu total organic carbon analyzer. The m-cresol conversion rate was determined using HPLC. The silicon concentration was determined using a spectrophotometer.
[0160] Example 8 The catalytic reaction conditions were optimized using the catalyst prepared in Example 1.
[0161] Intermittent catalytic ozone oxidation experiments were conducted using an intermittent reactor with a volume of 250 mL. Ozone was reacted with an ozone generator (CF-G-3-10g, Qingdao Guolin Environmental Protection Technology Co., Ltd.) to generate high-purity oxygen (99.999%). Rubber hoses were used to connect the inlet and outlet of the gas.
[0162] A 100 mg / L m-cresol and 500 mg / L silica-containing solution was prepared, and the pH was adjusted to 8.0. 2 g / L of the aforementioned anti-silica catalyst was then added to initiate the reaction. The ozone flow rate was set to 50 mL / min, the ozone concentration to 130 mg / L, and the reaction time to 60 min, according to the experimental conditions. The ozone was dispersed through the aeration head at the inlet and then introduced into the reaction solution.
[0163] During the reaction, a rotor was continuously stirred in the reactor at a speed of 1000 r / min. The reaction temperature was 20℃. Samples were periodically taken from the reactor to analyze the conversion rate of m-cresol, the removal rate of total organic carbon, and the anti-silicon performance of the catalyst. The results are shown in Table 2. The organic matter degradation performance of the samples was determined using a Shimadzu total organic carbon analyzer. The m-cresol conversion rate was determined using HPLC. The silicon concentration was determined using a spectrophotometer.
[0164] Table 2. Nitrogen carbide-modified perovskite catalysts (Sample 1#) Comparison of catalytic ozone oxidation and anti-silicon properties under different reaction conditions
[0165] Table 2 shows that different experimental conditions directly affect the experimental results. Under otherwise constant conditions, increasing the silicon concentration reduces the catalyst's anti-silicon performance. This is attributed to the fact that excessive silicon concentration makes the catalyst more susceptible to contact with silicon, thus adsorbing silicon species, but it has no significant effect on the removal efficiency (items 1-3). With increasing m-cresol concentration, the TOC removal rate and m-cresol conversion rate decrease (items 1, 4, 5). Regarding catalyst dosage, excessive catalyst dosage can promote the reaction effect. This is mainly because excessive catalyst can expose more active sites, thereby promoting the generation of free radicals and degrading pollutants (items 1, 6, 7). Regarding ozone concentration, with increasing ozone concentration, the catalyst reaction effect improves. This is mainly because more ozone can generate more free radicals, thus promoting the degradation of pollutants (items 1, 8, 9). Regarding reaction time, with increasing reaction time, the reaction becomes more complete (items 1, 10, 11). Regarding the pH value of the reaction, it can be seen that excessively acidic or alkaline conditions have an adverse effect on the reaction, while the reaction shows relatively excellent performance near the weakly alkaline condition of pH 8 (numbers 1, 12, and 13).
[0166] Example 9 The catalyst samples 1# to 3# were tested by transmission electron microscopy (TEM).
[0167] Taking sample 1# as a typical example, Figure 2 The image shows a transmission electron microscope (TEM) image of sample 1#. The coexistence of perovskite and nitrogen carbide can be observed in the image. The light-colored parts in the upper left and lower right of the image correspond to nitrogen carbide, while the dark-colored part in the upper right corresponds to perovskite. It can also be seen in the image that the perovskite has a lattice spacing of about 0.26 nm, corresponding to the (014) crystal plane. Nitrogen carbide plays a very important role in improving the anti-silicon properties of the catalyst.
[0168] Example 10 Scanning electron microscopy (SEM) was performed on catalyst samples 1# to 3# respectively. The results showed that catalyst samples 1# to 3# all exhibited a morphology of layered nitrogen carbide combined with spherical perovskite. Taking sample 1# as a typical example, Figure 3 The image shows a scanning electron microscope (SEM) image of sample 1#. As can be seen from the image, the catalyst has a sheet-like structure, which corresponds to sheet-like nitrogen carbide. At the same time, spherical particles are attached to the sheets, which corresponds to perovskite. The two form a heterostructure, constituting a nitrogen carbide-modified perovskite catalyst.
[0169] Example 11 Zeta potentials of catalyst samples 1 through 3 were measured using a nanoparticle size analyzer. The results showed that catalyst samples 1 through 3 exhibited a positive surface charge over a wider pH range. Taking sample 1# as a typical example, Figure 4 The figure shows the Zeta potential of sample 1#. It can be seen that the unmodified perovskite catalyst is positively charged at pH less than 5, while the modified catalyst is positively charged at pH less than 10. Since silicon in the substrate tends to be uncharged at pH 8, but a large number of hydroxide ions are present in the solution, these ions repel the negatively charged LFMO surface, leading to more silicon deposition on the LFMO surface. This coating of the catalyst's active sites hinders free radical generation. However, for the nitrogen carbide-modified perovskite catalyst, hydroxide ions more readily combine with the positively charged LFMO-CN-1 catalyst, generating oxygen-containing free radicals that degrade pollutants. This reduces the deposition of neutral silicon. Therefore, the nitrogen carbide-modified perovskite catalyst exhibits both excellent anti-silicon properties and high reactivity.
[0170] Example 12 X-ray diffraction (XRD) tests were performed on samples 1#~3# and comparative examples 1#~2# catalysts, respectively. The results showed that samples 1#~3# all exhibited characteristic peaks of perovskite and nitrogen carbide. Figure 5 The X-ray diffraction patterns of samples 1#~3# and comparative examples 1#~2# are shown. As can be seen from the patterns, the LFMO catalyst exhibits a diffraction peak at 32°, mainly attributed to the characteristic diffraction peaks of LaFeO3 (112) (01-074-2203) and LaMnO3 (104, 110) (01-089-8775). With increasing CN doping concentration, the characteristic diffraction peak of LFMO gradually weakens, while at 13°... and 27 The characteristic peaks that appear belong to the (100) and (022) planes of g-C3N4, which indicates that the catalyst has formed an LFMO-CN heterostructure. The heterostructure formed plays a very important role in improving the catalyst's anti-silicon properties and reaction activity.
[0171] Example 13 Nitrogen adsorption-desorption tests were performed on samples 1#~3# and comparative examples 1#~2# catalysts, respectively, using a nitrogen physical adsorption analyzer. The test results showed that samples 1#~3# catalysts all exhibited type IV isotherms; Figure 6 The nitrogen adsorption-desorption tests were performed on samples 1#~3# and comparative examples 1#~2# catalysts. The figure shows that the isotherms of the catalysts belong to type IV, and a significant hysteresis loop appears in the medium and high pressure region, indicating that the catalysts have a mesoporous structure and no macropores, which is conducive to the reaction of reactants on the catalyst surface.
[0172] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for treating silicon-containing organic wastewater by catalytic ozone oxidation, characterized in that, Includes the following steps: Silicon-containing organic wastewater is brought into contact with a catalyst and reacted in an ozone-containing atmosphere. The silicon-containing organic wastewater contains at least one of monosilicic acid, disilicic acid, and polysilicic acid. The catalyst is a nitrogen-carbon-modified perovskite anti-silicon catalyst, characterized in that... The nitrogen carbide-modified perovskite antisilicon catalyst comprises a nitrogen carbide layer and perovskite particles supported on the surface of the nitrogen carbide layer. The perovskite forms a heterostructure with layered nitrogen carbide; In the nitrogen carbide-modified perovskite antisilicon catalyst, the mass content of nitrogen carbide is 10~90 wt%; The perovskite particles loaded on the surface of the nitrogen carbide layer have a particle size of 30~80nm; The thickness of the nitride layer is 10~100 nm; The pore size of the nitrogen carbide-modified perovskite antisilicon catalyst is 8.9~14.9 nm; The specific surface area of the nitrogen-carbide modified perovskite silicon-resistant catalyst is 9-31 m 2 / g; The surface of the nitrogen-carbon-modified perovskite antisilicic catalysts described above is positively charged in the pH range of 3 to 10. The perovskite is of type AB perovskite; The A-site element of the perovskite is selected from at least one of La, Ca, and Sr; The B-site element of the perovskite is selected from at least one of Fe, Co, Ni, Mn, and Cu.
2. The method for treating silicon-containing organic wastewater by catalytic ozone oxidation according to claim 1, characterized in that, The lattice spacing of the perovskite particles loaded on the surface of the nitrogen carbide layer is 0.25~0.27 nm; The exposed crystal planes of the nitride layer are (100) and (022).
3. The method of claim 1, wherein the catalytic ozonation treatment of the silicon-containing organic wastewater is performed at a pH of 3 to 10. The nitrogen carbide-modified perovskite antisilicon catalyst is prepared by a method comprising the following steps: (1) Mix an aqueous solution containing precursor A and precursor B with an aqueous solution containing a precipitant, precipitate, age, dry, and calcine to obtain the perovskite; (2) The perovskite obtained in (1) is physically mixed with a nitrogen carbide source, dried and calcined to obtain the nitrogen carbide-modified perovskite anti-silicon catalyst; A is selected from at least one of La, Ca, and Sr; The B is selected from at least one of Fe, Co, Ni, Mn, and Cu.
4. The method of catalytic ozonation treatment of wastewater containing silicon organics according to claim 3, characterized in that, In the preparation method of the nitrogen carbide-modified perovskite antisilicon catalyst, The A precursor is selected from at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of La; at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of Ca; and at least one of the following: nitrate, sulfate, acetate, phosphate, and chloride of Sr. The B precursor is selected from at least one of the following: Fe nitrate, sulfate, acetate, phosphate, and chloride; Co nitrate, sulfate, acetate, phosphate, and chloride; Ni nitrate, sulfate, acetate, phosphate, and chloride; Mn nitrate, sulfate, acetate, phosphate, and chloride; and Cu nitrate, sulfate, acetate, phosphate, and chloride. In the aqueous solution containing precursor A and precursor B, the concentration of precursor A is 2-4 wt%, based on the mass of the metal element in precursor A; In the aqueous solution containing precursor A and precursor B, the concentration of precursor B is 0.5~1.2wt%, based on the mass of the metal element in precursor B; The volume ratio of the aqueous solution containing precursor A and precursor B to the aqueous solution containing the precipitant is 1:4 to 4:
1. The precipitant is selected from at least one of PEG1000, PEG2000, PEG4000, PEG6000, PEG10000, and PEG20000; In the aqueous solution containing the precipitant, the concentration of the precipitant is 0.1~1wt%; The mixing process controls the pH to be between 8 and 12.
5. The method of claim 3, wherein the catalytic ozonation treatment of the silicon-containing organic wastewater is performed at a pH of 3 to 10. In the preparation method of the nitrogen carbide-modified perovskite antisilicon catalyst, The precipitation temperature is 10~45℃; The precipitation time is 1-4 hours; The aging temperature is 70~100℃; The aging time is 12~48 hours; The drying temperature is 120~160℃; The drying time is 12-48 hours; The calcination temperature is 600~1000℃; The calcination time is 2 to 12 hours.
6. The method of claim 3, wherein the catalytic ozonation treatment of the silicon-containing organic wastewater is performed at a pH of 3 to 10. In the preparation method of the nitrogen carbide-modified perovskite antisilicon catalyst, The nitrogen carbide source is selected from at least one of melamine, dicyandiamide, and urea; The mass ratio of the perovskite obtained in (1) to the nitrogen carbide source is 9:1 to 1:9; The physical mixing includes grinding and stirring with water; The grinding time is 2-10 minutes; During the water addition and stirring process, the mass of water added is 2 to 20 times that of the nitrogen carbide source; The stirring time for adding water is 2 to 12 hours.
7. The method for treating silicon-containing organic wastewater by catalytic ozone oxidation according to claim 3, characterized in that, In the preparation method of the nitrogen carbide-modified perovskite antisilicon catalyst, The drying temperature is 50~100℃; The drying time is 10~48 hours; The roasting temperature is 300~600℃; The heating rate for calcination is 5~20℃ / min; The roasting time is 2-8 hours; The calcination atmosphere is a non-reactive gas atmosphere; The inactive gas atmosphere is selected from at least one of nitrogen, helium, and argon.
8. The method for treating silicon-containing organic wastewater by catalytic ozone oxidation according to claim 1, characterized in that, The silicon content in the silicon-containing organic wastewater is 10~500 mg / L; based on the mass of silicon dioxide; The silicon-containing organic wastewater also contains at least one of m-cresol, o-cresol, p-cresol, maleic acid, acetic acid, bisphenol A, bisphenol F, and acrylic acid.
9. The method for treating silicon-containing organic wastewater by catalytic ozone oxidation according to claim 1, characterized in that, The reaction temperature is 10~30℃; The reaction time is 10-120 min; In the ozone-containing atmosphere, the ozone concentration is 50~200 mg / L; In the ozone-containing atmosphere, the ozone flow rate is 20~80 mL / min; The mass ratio of the catalyst to the solid-liquid mixture of the silicon-containing organic wastewater is 0.5~5 g / L; The pH is controlled at 3-11 during the reaction process.
Citation Information
Patent Citations
Preparation method of mesoporous carbon nitride loaded precious nano particle
CN102931418B
Graphite-phase carbon nitride (g-C3N4) material and preparation method and application thereof
CN105126893A
A preparing method of a nitrogen carbide material
CN105731397A
A solar cell material
CN106229412B
A method for preparing nanoporous graphitic nitrogen carbide materials and their applications
CN107029774B