A high-strength and tough welding electrode for welding high-pressure hydrogen storage pressure vessels and its preparation method

By combining a high-purity, high-strength welding core with a low-hydrogen, alkaline coating, the problem of insufficient weld strength and toughness in the welding of large-capacity, high-pressure hydrogen storage vessels has been solved. This has resulted in welding electrodes with high strength, low hydrogen content, and excellent welding performance, meeting the production requirements of high-pressure hydrogen storage vessels.

CN118060787BActive Publication Date: 2026-11-10CHINA NAT PETROLEUM CORP +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211468439.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2026-11-10
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

Existing technologies lack high-strength and tough welding electrodes that can meet the welding requirements of large-capacity high-pressure hydrogen storage vessels, especially the low-temperature toughness of welds with tensile strengths above 800MPa, which makes it difficult to produce high-pressure hydrogen storage vessels of the 100 cubic meter level.

Method used

The welding electrode employs a combination design of high-purity, high-strength core material and low-hydrogen alkaline coating. The core material consists of C, Si, Mn, Ni, Cr, Mo, Ti, and B, while the coating consists of marble, fluorite, barium carbonate, quartz sand, titanium dioxide, zircon sand, rare earth ferrosilicon, and reduced iron powder. Through solid solution strengthening, fine grain strengthening, and the strengthening effect of microalloying element precipitates, combined with optimized electrode preparation process, the high strength and low-temperature toughness of the weld are ensured.

Benefits of technology

The weld has a tensile strength of over 800MPa, an impact energy of over 100J at -40℃, a diffusible hydrogen content of less than 4ml/100g, a stable welding process, and an aesthetically pleasing weld morphology, meeting the welding requirements for large-capacity, high-pressure hydrogen storage pressure vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118060787B_ABST
    Figure CN118060787B_ABST
Patent Text Reader

Abstract

This invention discloses a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels and its preparation method. Through a reasonable design of the core and coating composition, the weld metal achieves a Mn-Si-Ni-Cr-Mo-Ti-B alloy system. Utilizing the strengthening effects of solid solution strengthening, fine grain strengthening, and microalloying element precipitates, the electrode ensures high strength of the weld metal while preventing the formation of hardened structures, thus improving the weld's crack resistance. Employing a high-purity, high-strength core and a low-hydrogen alkaline slag system, along with high-quality coating powder with low S and P content, the electrode exhibits excellent all-position welding process performance and mechanical properties. The welding process results in minimal spatter, aesthetically pleasing weld bead morphology, and no slag adhesion. After heat treatment at 580℃ for 2 hours, the weld metal achieves a tensile strength of over 800 MPa, an elongation of ≥18%, an impact energy of over 100 J at -40℃, and a diffusible hydrogen content of less than 4 ml / 100g, meeting the welding requirements of large-capacity high-pressure hydrogen storage pressure vessels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of welding materials technology, specifically to a high-strength and tough welding electrode for welding high-pressure hydrogen storage pressure vessels and its preparation method. Background Technology

[0002] To address the severe reality of global warming, achieving low-carbon and decarbonized development of the energy system is imperative. Hydrogen energy, due to its wide availability and clean, safe characteristics, has become an important carrier of green energy. Currently, major world powers are investing heavily in actively promoting the development of the hydrogen energy industry, vying for a leading position in the hydrogen energy competition.

[0003] In the process of hydrogen production and use, large-capacity and safe hydrogen storage has become a major requirement in the hydrogen energy industry. High-pressure hydrogen storage vessels, such as fixed, thick-walled spherical hydrogen storage tanks, can realize large-capacity hydrogen storage in hydrogen production plants or hydrogen refueling stations. However, due to the shortage of welding materials, China has not yet successfully developed a large-capacity, high-pressure gaseous hydrogen storage vessel with a capacity of hundreds of cubic meters.

[0004] Currently, research and application of welding electrodes for hydrogen storage tanks in my country mainly focus on tensile strength levels of 500–700 MPa, resulting in excellent low-temperature toughness of the weld. Research and application of electrodes with tensile strengths above 800 MPa primarily focus on high-strength steel, prioritizing tensile strength, but generally resulting in low-temperature impact toughness of the weld. Research on hydrogen-resistant, high-strength, and high-toughness welding electrodes with a weld metal tensile strength ≥800 MPa and an impact absorption energy ≥100 J at -40℃ for high-pressure hydrogen storage vessels at the 100 cubic meter level is still lacking, and the development of related high-end welding materials is urgently needed. Summary of the Invention

[0005] To address the problems existing in the prior art, this invention provides a high-strength and tough welding electrode for welding high-pressure hydrogen storage pressure vessels and its preparation method, which enables the production and manufacturing of large-capacity, low-cost single-layer steel high-pressure hydrogen storage pressure vessels for hydrogen production plants and hydrogen refueling stations.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] A high-strength and tough welding electrode for welding high-pressure hydrogen storage pressure vessels includes a core and a coating.

[0008] The coating accounts for 35% to 45% of the total weight of the electrode, and the core material accounts for 55% to 65% of the total weight of the electrode.

[0009] The core material, by mass fraction, is: C: 0.04%–0.08%; Si: 0.4%–0.6%; Mn: 1.4%–1.6%; Ni: 1.3%–1.8%; Cr: 0.1%–0.15%; Mo: 0.1%–0.2%; Ti: 0.04%–0.08%; B: 0.004%–0.007%; S≤0.005%; P≤0.008%; the balance is Fe.

[0010] The components of the coating, by mass fraction, are: marble: 27%–35%; fluorite: 13%–18%; barium carbonate: 7%–9%; quartz sand: 4%–7%; titanium dioxide: 3%–5%; zircon sand: 2%–3%; rare earth ferrosilicon: 3%–5%; ferromanganese: 4%–6%; reduced iron powder: 13%–18%; soda ash: 1%–2%.

[0011] Preferably, the w(Mn) / w(Si) ratio in the welding core is between 2.5 and 4.5, the w(Mn) / w(Ni) ratio is between 0.7 and 1.4, and the w(Ti) / w(B) ratio is between 5 and 10.

[0012] Preferably, the diameter deviation range of the welding core is ±0.3mm.

[0013] Preferably, the alkalinity of the drug coating is 2.8 to 3.5.

[0014] Preferably, the w(marble) / w(fluorite) ratio in the coating is between 1.6 and 2.1, the w(titanium dioxide) / w(zircon sand) ratio is between 1.5 and 2.5, and the w(manganese iron) / w(rare earth silicon iron) ratio is between 1 and 2.

[0015] Preferably, the composition and particle size of each powder in the coating are as follows: Marble: CaCO3 ≥ 98%, 40 mesh; Fluorite: CaF2 ≥ 96%, 40 mesh; Barium carbonate: BaCO3 ≥ 80%, 40 mesh; Quartz sand: SiO2 ≥ 99%, 40 mesh; Titanium dioxide: TiO2 ≥ 98%, 40 mesh; Zircon sand: ZrO2 ≥ 99%, 40 mesh; Rare earth ferrosilicon: Re ≥ 30%, Si ≥ 45%, 60 mesh; Ferromanganese: Mn ≥ 75%, 80 mesh; Reduced iron powder: Fe ≥ 98%, 80 mesh; Soda ash: Na2CO3 ≥ 99.2%, 200 mesh.

[0016] A method for preparing a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage vessels includes the following steps:

[0017] After annealing and heat treatment, the core wire is drawn with reduced diameter, then leveled and cut to form the core. The core contains the following components by mass fraction: C: 0.04%–0.08%; Si: 0.4%–0.6%; Mn: 1.4%–1.6%; Ni: 1.3%–1.8%; Cr: 0.1%–0.15%; Mo: 0.1%–0.2%; Ti: 0.04%–0.08%; B: 0.004%–0.007%; S≤0.005%; P≤0.008%; the balance is Fe.

[0018] The powdered medicinal materials are mixed together, and the components of the medicinal materials, by mass fraction, are: marble: 27%–35%; fluorite: 13%–18%; barium carbonate: 7%–9%; quartz sand: 4%–7%; titanium dioxide: 3%–5%; zircon sand: 2%–3%; rare earth ferrosilicon: 3%–5%; ferromanganese: 4%–6%; reduced iron powder: 13%–18%; soda ash: 1%–2%.

[0019] Water glass is added to the mixed drug coating powder, and after mixing evenly, a drug coating material is formed.

[0020] The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0021] Wet welding electrodes are dried to form high-strength and tough welding electrodes for welding high-pressure hydrogen storage pressure vessels.

[0022] Preferably, the annealing process of the welding core wire is controlled at 690±10℃×2h, and the single compression ratio range of the welding core wire drawing process is 9%~13%.

[0023] Preferably, when wet-mixing the drug coating powder, potassium sodium water glass with a modulus M of 3.1 and a Baume degree (20°C) of 38-40°Bé is used.

[0024] Preferably, a segmented drying method is used when drying wet welding rods. After the wet welding rods are naturally dried at room temperature for 8 hours, they are dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0025] Compared with the prior art, the present invention has the following beneficial technical effects:

[0026] This invention discloses a low-hydrogen, high-strength, and high-toughness welding electrode for welding large-capacity, high-pressure hydrogen storage pressure vessels. Through a rational design of the core and coating composition, the weld metal achieves a Mn-Si-Ni-Cr-Mo-Ti-B alloy system. Utilizing the strengthening effects of solid solution strengthening, fine grain strengthening, and microalloying element precipitation, the electrode ensures high strength of the weld metal while preventing the formation of hardened structures, thus improving the weld's crack resistance. Employing a high-purity, high-strength core and a low-hydrogen alkaline slag system, along with high-quality coating powder with low S and P content, the electrode exhibits excellent all-position welding process performance and mechanical properties. The welding process results in minimal spatter, aesthetically pleasing weld bead morphology, and no slag adhesion. After heat treatment at 580℃ for 2 hours, the weld metal achieves a tensile strength of over 800 MPa, an elongation of ≥18%, an impact energy of over 100 J at -40℃, and a diffusible hydrogen content of less than 4 ml / 100g, meeting the welding requirements of large-capacity, high-pressure hydrogen storage pressure vessels. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the metallographic structure (AF+B) of the electrode deposited metal in an embodiment. Detailed Implementation

[0028] The present invention will be further described in detail below with reference to specific embodiments. These descriptions are for explanation purposes only and are not intended to limit the scope of the invention.

[0029] This invention discloses a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels, comprising a special high-purity, high-strength core and a coating. The coating comprises approximately 35% to 45% of the total weight of the electrode. The coating includes powdered raw materials and a binder; when the coating powder is wet-mixed, the binder comprises approximately 16% to 19% of the total weight of the coating. Alloying elements are transferred jointly by the high-strength core and the coating.

[0030] Specialized high-purity, high-strength, and high-toughness welding cores and optimized welding core manufacturing processes. The chemical composition of the welding core, by mass fraction, is as follows: C: 0.04%–0.08%; Si: 0.4%–0.6%; Mn: 1.4%–1.6%; Ni: 1.3%–1.8%; Cr: 0.1%–0.15%; Mo: 0.1%–0.2%; Ti: 0.04%–0.08%; B: 0.004%–0.007%; S≤0.005%; P≤0.008%; balance Fe. The welding core chemical composition must simultaneously meet the following requirements: w(Mn) / w(Si) ratio 2.5–4.5, w(Mn) / w(Ni) ratio 0.7–1.4, and w(Ti) / w(B) ratio 5–10. The annealing process of the core wire rod is controlled at 690±10℃×2h, the single compression ratio of the core wire rod drawing process is controlled at 9%~13%, and the diameter deviation of the finished core wire rod is controlled at ±0.3mm.

[0031] Low-hydrogen alkaline welding electrode coating and preferred coating powder. The coating composition, by mass fraction, is as follows: marble: 27%–35%; fluorite: 13%–18%; barium carbonate: 7%–9%; quartz sand: 4%–7%; titanium dioxide: 3%–5%; zircon sand: 2%–3%; rare earth ferrosilicon: 3%–5%; ferromanganese: 4%–6%; reduced iron powder: 13%–18%; soda ash: 1%–2%. The basicity of the electrode coating is 2.8–3.5. The coating composition must simultaneously meet the following requirements: w(marble) / w(fluorite) ratio is 1.6–2.1, w(titanium dioxide) / w(zircon sand) ratio is 1.5–2.5, and w(ferromanganese) / w(rare earth ferrosilicon) ratio is 1–2. The main chemical components and particle size requirements for the powder are as follows: Marble: CaCO3 ≥ 98%, 40 mesh; Fluorite: CaF2 ≥ 96%, 40 mesh; Barium carbonate: BaCO3 ≥ 80%, 40 mesh; Quartz sand: SiO2 ≥ 99%, 40 mesh; Titanium dioxide: TiO2 ≥ 98%, 40 mesh; Zircon sand: ZrO2 ≥ 99%, 40 mesh; Rare earth ferrosilicon: Re ≥ 30%, Si ≥ 45%, 60 mesh; Ferromanganese: Mn ≥ 75%, 80 mesh; Reduced iron powder: Fe ≥ 98%, 80 mesh; Soda ash: Na2CO3 ≥ 99.2%, 200 mesh.

[0032] This invention provides an optimized electrode preparation process. During the wet mixing of the flux powder, potassium-sodium silicate with a modulus M of 3.1 and a Baume degree (20°C) of 38–40°Bé is used. For electrode drying, a segmented drying process is employed: after natural drying at room temperature for 8 hours, a subsequent drying process of 150°C × 2h → 300°C × 2h → 450°C × 2h is used.

[0033] This invention, through a rational design of the core and coating composition, achieves a Mn-Si-Ni-Cr-Mo-Ti-B alloy system in the weld metal. Utilizing solid solution strengthening, grain refinement strengthening, and the strengthening effect of microalloying element precipitates, it ensures high strength of the weld metal while preventing the formation of hardened structures, thus improving the weld's crack resistance. The weld metal in the heat-treated state (580℃×2h) has a tensile strength ≥800MPa, elongation ≥18%, and impact energy at -40℃ ≥100J. ① Mn and Si elements act as deoxidizers and desulfurizers, also playing a role in solid solution strengthening, which is beneficial to improving the strength and toughness of the weld metal. ② Ni element can promote the formation of acicular ferrite, lower the ductile-brittle transition temperature of the weld metal, and improve impact toughness. ③ When the w(Mn) / w(Si) ratio of the weld metal is between 2.5 and 4.5, and the w(Mn) / w(Ni) ratio is between 0.9 and 1.5, the weld metal exhibits good strength and toughness. ④ Cr and Mo elements can lower the austenite transformation temperature, inhibit the formation of proeutectoid ferrite, and shift the phase transformation towards the acicular ferrite temperature range, which is beneficial for microstructure refinement. However, their content should not exceed 1.0%, otherwise it will promote the formation of MA components, leading to hot cracking in the weld. ⑤ Ti elements readily form strong carbides / nitrides and pin them to grain boundaries, effectively preventing austenite grain growth while providing nucleation sites for acicular ferrite, thus promoting its formation. ⑥ Boron elements can rapidly diffuse to the austenite grain boundaries during welding cooling, forming fine boron phases coherent with austenite, reducing the grain boundary interface energy, inhibiting the precipitation of proeutectoid ferrite, and promoting the nucleation and growth of intragranular acicular ferrite on borides. ⑦ When the w(Ti) / w(B) ratio of the deposited metal is between 5 and 10, the content of acicular ferrite in the deposited metal is significantly increased.

[0034] This invention, through a rational design of the flux coating composition, achieves a low-hydrogen, high-basicity slag system of CaO-CaF2-BaO-SiO2-TiO2-ZrO2. This results in a stable arc, easy slag removal, aesthetically pleasing weld bead formation, and good all-position welding performance during the welding process. Furthermore, optimized drying processes ensure that the diffusible hydrogen content in the weld metal is ≤4ml / 100g, leading to a low rate of cold cracking in the weld. ① Marble and barium carbonate are the main arc stabilizers, slag-forming agents, and gas-generating agents. CaCO3 decomposes into CaO+CO2 at high arc temperatures. The CO2 gas helps increase arc blowing force and improve arc stiffness. The low ionization potential of Ca and Ba ions enhances arc stability. Fluorite, quartz sand, and zircon sand are the main slag-forming agents and diluents. Ferromanganese and rare-earth ferrosilicon are the main deoxidizers and alloying agents, preventing oxidation of the weld metal. Simultaneously, Mn and S can form MnS, providing a certain degree of desulfurization. Titanium dioxide and soda ash are the main plasticizers, making the welding electrodes easier to shape during production. ② During welding, the components of the electrode coating react interactively after melting, achieving stable arc combustion, slag-gas protection of the weld pool, and metallurgical reaction. ③ When the w(marble) / w(fluorite) ratio is between 1.6 and 2.1, the arc break length reaches over 22 mm, significantly improving arc stability and slag removal. ④ When the zircon sand content is between 2% and 3%, slag removal performance is significantly improved. When the w(titanium dioxide) / w(zircon sand) ratio is between 1.5 and 2.5, the spatter rate is significantly reduced.

[0035] This invention refines the weld microstructure by rationally adding 3%–5% rare earth ferrosilicon to the electrode coating, achieving an acicular ferrite (AF) content of over 90%; it also improves weld toughness, with an impact energy exceeding 100J at -40℃. The addition of rare earth elements isolates harmful elements such as sulfur (S) and phosphorus (P) outside the grain boundaries and forms spherical rare earth oxides, inhibiting grain boundary growth and refining grains. When the rare earth ferrosilicon content is between 0% and 5%, the weld impact energy increases with increasing rare earth ferrosilicon content; however, as the rare earth ferrosilicon content continues to increase, the weld impact energy shows no significant change, and slag adhesion occurs. Simultaneously, ferrosilicon itself has deoxidizing properties, protecting alloying elements in the molten pool and contributing to improved weld strength and toughness.

[0036] This invention improves slag fluidity and increases electrode deposition efficiency to 110% by rationally adding 13%–18% reduced iron powder to the electrode coating, thereby increasing electrode utilization and construction efficiency. Electrode deposition efficiency is defined as the ratio of the mass of the deposited metal formed after welding to the nominal mass of the melted core. After the electrode melts, most of the core material forms deposited metal, but some core material is burned off during complex molten pool reactions and enters the slag shell. Therefore, the deposition rate of ordinary electrodes is generally below 100%. When the reduced iron powder content is further increased to over 15%, the electrode deposition efficiency continues to improve, but the all-position welding process performance deteriorates.

[0037] This invention optimizes the heat treatment and drawing process of the welding core wire rod, resulting in a welding core with moderate hardness, high roundness, and good geometric dimensional uniformity. After leveling and coating, the resulting welding electrode exhibits low eccentricity, ensuring stable welding process. Electrode eccentricity leads to uneven melting rates of the electrode coating during welding, preventing the formation of a proper sleeve, causing arc blow and arc instability, and affecting welding quality.

[0038] Example 1

[0039] In this embodiment, approximately 100 kg of welding rods are prepared on the production line. The raw materials used are 60 kg of special high-purity, high-strength and tough welding core, 40 kg of alkaline flux powder, 8 kg of potassium sodium water glass, and the welding rod specifications are Φ4.0 mm × 400 mm.

[0040] The chemical composition of the special high-purity, high-strength and high-toughness welding core used in this embodiment is as follows: C: 0.061%; Si: 0.52%; Mn: 1.48%; Ni: 1.66%; Cr: 0.10%; Mo: 0.10%; Ti: 0.043%; B: 0.0065%; S: 0.003%; P: 0.005%; with the balance being Fe.

[0041] In this embodiment, the amounts of each component added when preparing the drug coating powder are as follows: marble: 13.9 kg; fluorite: 6.0 kg; barium carbonate: 3.6 kg; quartz sand: 2.7 kg; titanium dioxide: 1.9 kg; zircon sand: 0.9 kg; rare earth ferrosilicon: 1.6 kg; ferromanganese: 1.6 kg; reduced iron powder: 7.2 kg; soda ash: 0.6 kg. This embodiment uses potassium-sodium water glass with a modulus M of 3.1 and a Baume degree (20°C) of 40°Bé.

[0042] The main preparation process of the welding electrode in this embodiment is as follows:

[0043] (1) Core processing: After the wire rod arrives, it is annealed at 690±10℃ for 2 hours. After peeling and pickling, it is drawn in the order of Φ5.5mm→Φ5.0mm→Φ4.5mm→Φ4.0mm (core diameter range is 4.01~4.20mm). Then, the core is straightened and cut on a straightening and cutting machine (cut at 400mm / piece).

[0044] (2) Dry mixing of drug peel: Weigh the drug peel powder according to the above proportions and mix it evenly in a mixer.

[0045] (3) Wet mixing of drug coating: Add small amounts of the aforementioned water glass into the mixer multiple times and mix it evenly with the drug coating powder to form a drug coating with a certain viscosity.

[0046] (4) Electrode coating: The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0047] (5) Electrode drying: An optimized segmented drying method is adopted. After the wet electrode is naturally dried at room temperature for 8 hours, it is dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0048] After the welding electrodes were prepared, welding tests and performance evaluations of the deposited metal were conducted according to the test methods specified in GB / T 39281-2020. In this embodiment, the welding process exhibited a stable arc, minimal spatter, aesthetically pleasing weld formation, easy slag removal, and excellent weld operability. The chemical composition of the deposited metal is shown in Table 1, and the mechanical properties are shown in Table 2. The diffusible hydrogen content of the deposited metal was 3.2 ml / 100 g.

[0049] Table 1 Chemical composition of the weld metal deposited by the electrode in Example 1 (wt, %)

[0050] element C Si Mn P S Ni Cr Mo Ti B content 0.062 0.63 1.78 0.006 0.005 1.48 0.05 0.08 0.032 0.0052

[0051] Table 2 Mechanical properties of weld metal deposited by electrode in Example 1 (wt, %)

[0052]

[0053] Example 2

[0054] In this embodiment, approximately 100 kg of welding rods are prepared on the production line. The raw materials used are 60 kg of special high-purity, high-strength and tough welding core, 40 kg of alkaline flux powder, 8.2 kg of potassium sodium water glass, and the welding rod specifications are Φ4.0 mm × 400 mm.

[0055] The chemical composition of the special high-purity, high-strength and high-toughness welding core used in this embodiment is as follows: C: 0.068%; Si: 0.6%; Mn: 1.4%; Ni: 1.8%; Cr: 0.10%; Mo: 0.15%; Ti: 0.05%; B: 0.0065%; S: 0.004%; P: 0.005%; with the balance being Fe.

[0056] In this embodiment, the amounts of each component added when preparing the drug coating powder are as follows: marble: 13.2 kg; fluorite: 6.4 kg; barium carbonate: 3.3 kg; quartz sand: 2.5 kg; titanium dioxide: 1.8 kg; zircon sand: 1.2 kg; rare earth ferrosilicon: 1.9 kg; ferromanganese: 2.4 kg; reduced iron powder: 6.9 kg; soda ash: 0.4 kg. This embodiment uses potassium-sodium silicate with a modulus M of 3.1 and a Baume degree (20°C) of 40°Bé.

[0057] The main preparation process of the welding electrode in this embodiment is as follows:

[0058] (1) Core processing: After the wire rod arrives, it is annealed at 690±10℃ for 2 hours. After peeling and pickling, it is drawn in the order of Φ5.5mm→Φ5.0mm→Φ4.5mm→Φ4.0mm (core diameter range is 4.05~4.15mm). Then, the core is straightened and cut on a straightening and cutting machine (cut at 400mm / piece).

[0059] (2) Dry mixing of drug peel: Weigh the drug peel powder according to the above proportions and mix it evenly in a mixer.

[0060] (3) Wet mixing of drug coating: Add small amounts of the aforementioned water glass into the mixer multiple times and mix it evenly with the drug coating powder to form a drug coating with a certain viscosity.

[0061] (4) Electrode coating: The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0062] (5) Electrode drying: An optimized segmented drying method is adopted. After the wet electrode is naturally dried at room temperature for 8 hours, it is dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0063] After the welding electrodes were prepared, welding tests and performance evaluations of the deposited metal were conducted according to the test methods specified in GB / T 39281-2020. In this embodiment, the welding process exhibited a stable arc, minimal spatter, aesthetically pleasing weld formation, easy slag removal, and excellent weld operability. The chemical composition of the deposited metal is shown in Table 3, and its mechanical properties are shown in Table 4. The diffusible hydrogen content of the deposited metal was 3.0 ml / 100 g.

[0064] Table 3 Chemical composition of the weld metal deposited by the welding electrode in Example 2 (wt, %)

[0065] element C Si Mn P S Ni Cr Mo Ti B content 0.065 0.62 1.65 0.006 0.005 1.52 0.04 0.07 0.031 0.0053

[0066] Table 4 Mechanical properties of weld metal deposited by electrode in Example 2 (wt, %)

[0067]

[0068] Example 3

[0069] In this embodiment, approximately 100 kg of welding rods are prepared on the production line. The raw materials used are 55 kg of special high-purity, high-strength and tough welding core, 45 kg of alkaline flux powder, 8.0 kg of potassium sodium water glass, and the welding rod specifications are Φ4.0 mm × 400 mm.

[0070] The chemical composition of the special high-purity, high-strength and high-toughness welding core used in this embodiment is as follows: C: 0.04%; Si: 0.53%; Mn: 1.52%; Ni: 1.3%; Cr: 0.12%; Mo: 0.13%; Ti: 0.04%; B: 0.004%; S: 0.004%; P: 0.005%; with the balance being Fe.

[0071] In this embodiment, the amounts of each component added when preparing the drug coating powder are as follows: marble: 14 kg; fluorite: 7.5 kg; barium carbonate: 3.8 kg; quartz sand: 2.9 kg; titanium dioxide: 2.2 kg; zircon sand: 1.4 kg; rare earth ferrosilicon: 2.4 kg; ferromanganese: 2.5 kg; reduced iron powder: 7.5 kg; soda ash: 0.8 kg. This embodiment uses potassium-sodium silicate with a modulus M of 3.1 and a Baume degree (20°C) of 40°Bé.

[0072] The main preparation process of the welding electrode in this embodiment is as follows:

[0073] (1) Core processing: After the wire rod arrives, it is annealed at 690±10℃ for 2 hours. After peeling and pickling, it is drawn in the order of Φ5.5mm→Φ5.0mm→Φ4.5mm→Φ4.0mm (core diameter range is 4.00~4.15mm). Then, the core is straightened and cut on a straightening and cutting machine (cut at 400mm / piece).

[0074] (2) Dry mixing of drug peel: Weigh the drug peel powder according to the above proportions and mix it evenly in a mixer.

[0075] (3) Wet mixing of drug coating: Add small amounts of the aforementioned water glass into the mixer multiple times and mix it evenly with the drug coating powder to form a drug coating with a certain viscosity.

[0076] (4) Electrode coating: The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0077] (5) Electrode drying: An optimized segmented drying method is adopted. After the wet electrode is naturally dried at room temperature for 8 hours, it is dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0078] After the welding electrodes were prepared, welding tests and performance evaluations of the deposited metal were conducted according to the test methods specified in GB / T 39281-2020. In this embodiment, the welding process exhibited a stable arc, minimal spatter, aesthetically pleasing weld formation, easy slag removal, and excellent weld operability. The chemical composition of the deposited metal is shown in Table 5, and the mechanical properties are shown in Table 6. The diffusible hydrogen content of the deposited metal was 3.2 ml / 100 g.

[0079] Table 5 Chemical composition of the weld metal deposited by the electrode in Example 3 (wt, %)

[0080] element C Si Mn P S Ni Cr Mo Ti B content 0.60 0.62 1.7 0.006 0.005 1.48 0.06 0.06 0.035 0.0032

[0081] Table 6 Mechanical properties of weld metal deposited by electrode in Example 3 (wt, %)

[0082]

[0083] Example 4

[0084] In this embodiment, approximately 100 kg of welding rods are prepared on the production line. The raw materials used are 65 kg of special high-purity, high-strength and tough welding core, 35 kg of alkaline flux powder, 8.5 kg of potassium sodium water glass, and the welding rod specifications are Φ4.0 mm × 400 mm.

[0085] The chemical composition of the special high-purity, high-strength and high-toughness welding core used in this embodiment is as follows: C: 0.065%; Si: 0.4%; Mn: 1.6%; Ni: 1.58%; Cr: 0.15%; Mo: 0.2%; Ti: 0.048%; B: 0.005%; S: 0.003%; P: 0.005%; with the balance being Fe.

[0086] In this embodiment, the amounts of each component added when preparing the drug coating powder are as follows: marble: 12.0 kg; fluorite: 6.0 kg; barium carbonate: 2.5 kg; quartz sand: 1.6 kg; titanium dioxide: 1.8 kg; zircon sand: 0.7 kg; rare earth ferrosilicon: 1.2 kg; ferromanganese: 2.2 kg; reduced iron powder: 6.4 kg; soda ash: 0.6 kg. This embodiment uses potassium sodium silicate with a modulus M of 3.1 and a Baume degree (20°C) of 40°Bé.

[0087] The main preparation process of the welding electrode in this embodiment is as follows:

[0088] (1) Core processing: After the wire rod arrives, it is annealed at 690±10℃ for 2 hours. After peeling and pickling, it is drawn in the order of Φ5.5mm→Φ5.0mm→Φ4.5mm→Φ4.0mm (core diameter range is 4.05~4.18mm). Then, the core is straightened and cut on a straightening and cutting machine (cut at 400mm / piece).

[0089] (2) Dry mixing of drug peel: Weigh the drug peel powder according to the above proportions and mix it evenly in a mixer.

[0090] (3) Wet mixing of drug coating: Add small amounts of the aforementioned water glass into the mixer multiple times and mix it evenly with the drug coating powder to form a drug coating with a certain viscosity.

[0091] (4) Electrode coating: The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0092] (5) Electrode drying: An optimized segmented drying method is adopted. After the wet electrode is naturally dried at room temperature for 8 hours, it is dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0093] After the welding electrodes were prepared, welding tests and performance evaluations of the deposited metal were conducted according to the test methods specified in GB / T 39281-2020. In this embodiment, the welding process exhibited a stable arc, minimal spatter, aesthetically pleasing weld formation, easy slag removal, and excellent weld operability. The chemical composition of the deposited metal is shown in Table 7, and the mechanical properties are shown in Table 8. The diffusible hydrogen content of the deposited metal was 3.3 ml / 100 g.

[0094] Table 7 Chemical composition (wt, %) of the weld metal deposited by the electrode in Example 4

[0095] element C Si Mn P S Ni Cr Mo Ti B content 0.69 0.58 1.67 0.006 0.005 1.45 0.06 0.0 0.035 0.0037

[0096] Table 8 Mechanical properties of weld metal deposited by electrode in Example 4 (wt, %)

[0097]

[0098] Example 5

[0099] In this embodiment, approximately 100 kg of welding rods are prepared on the production line. The raw materials used are 60 kg of special high-purity, high-strength and tough welding core, 40 kg of alkaline flux powder, 7.9 kg of potassium sodium water glass, and the welding rod specifications are Φ4.0 mm × 400 mm.

[0100] The chemical composition of the special high-purity, high-strength and high-toughness welding core used in this embodiment is as follows: C: 0.8%; Si: 0.48%; Mn: 1.52%; Ni: 1.62%; Cr: 0.1%; Mo: 0.15%; Ti: 0.08%; B: 0.007%; S: 0.003%; P: 0.005%; with the balance being Fe.

[0101] In this embodiment, the amounts of each component added when preparing the drug coating powder are as follows: marble: 14.0 kg; fluorite: 7.1 kg; barium carbonate: 3.5 kg; quartz sand: 2.1 kg; titanium dioxide: 1.6 kg; zircon sand: 1.0 kg; rare earth ferrosilicon: 2.0 kg; ferromanganese: 2.0 kg; reduced iron powder: 6.0 kg; soda ash: 0.7 kg. This embodiment uses potassium-sodium silicate with a modulus M of 3.1 and a Baume degree (20°C) of 40°Bé.

[0102] The main preparation process of the welding electrode in this embodiment is as follows:

[0103] (1) Core processing: After the wire rod arrives, it is annealed at 690±10℃ for 2 hours. After peeling and pickling, it is drawn in the order of Φ5.5mm→Φ5.0mm→Φ4.5mm→Φ4.0mm (core diameter range is 4.05~4.20mm). Then, the core is straightened and cut on a straightening and cutting machine (cut at 400mm / piece).

[0104] (2) Dry mixing of drug peel: Weigh the drug peel powder according to the above proportions and mix it evenly in a mixer.

[0105] (3) Wet mixing of drug coating: Add small amounts of the aforementioned water glass into the mixer multiple times and mix it evenly with the drug coating powder to form a drug coating with a certain viscosity.

[0106] (4) Electrode coating: The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode.

[0107] (5) Electrode drying: An optimized segmented drying method is adopted. After the wet electrode is naturally dried at room temperature for 8 hours, it is dried using a process of 150℃×2h→300℃×2h→450℃×2h.

[0108] After the welding electrodes were prepared, welding tests and performance evaluations of the deposited metal were conducted according to the test methods specified in GB / T 39281-2020. In this embodiment, the welding process exhibited a stable arc, minimal spatter, aesthetically pleasing weld formation, easy slag removal, and excellent weld operability. The chemical composition of the deposited metal is shown in Table 9, and its mechanical properties are shown in Table 10. The diffusible hydrogen content of the deposited metal was 3.0 ml / 100 g.

[0109] Table 9 Chemical composition (wt, %) of the weld metal deposited by the electrode in Example 5

[0110] element C Si Mn P S Ni Cr Mo Ti B content 0.72 0.55 1.7 0.006 0.005 1.52 0.05 0.06 0.043 0.0058

[0111] Table 10 Mechanical properties of weld metal deposited by electrode in Example 5 (wt, %)

[0112]

Claims

1. A high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels, characterized in that, Including the core and the flux coating; The coating comprises 35% to 45% of the total weight of the welding electrode, and the core comprises 55% to 65% of the total weight of the welding electrode. The welding core, by mass fraction, is: C: 0.04%~0.08%; Si: 0.4%~0.6%; Mn: 1.4%~1.6%; Ni: 1.3%~1.8%; Cr: 0.1%~0.15%; Mo: 0.1%~0.2%; Ti: 0.04%~0.08%; B: 0.004%~0.007%; S≤0.005%; P≤0.008%; balance Fe; The components of the medicinal coating, by mass fraction, are: marble: 27%~35%; Fluorite: 13%~18%; Barium carbonate: 7%~9%; Quartz sand: 4%~7%; Titanium dioxide: 3%~5%; Zircon sand: 2%~3%; Rare earth ferrosilicon: 3%~5%; Ferromanganese: 4%~6%; Reduced iron powder: 13%~18%; Soda ash: 1%~2%; The w(Mn) / w(Si) ratio in the core is between 2.5 and 4.5, the w(Mn) / w(Ni) ratio is between 0.7 and 1.4, and the w(Ti) / w(B) ratio is between 5 and 10. The alkalinity of the drug coating is 2.8~3.5; The ratio of w(marble) to w(fluorite) in the coating is between 1.6 and 2.1, the ratio of w(titanium dioxide) to w(zircon sand) is between 1.5 and 2.5, and the ratio of w(ferromanganese) to w(ferrosilicon rare earth) is between 1 and 2.

2. The high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels according to claim 1, characterized in that, The diameter deviation range of the welding core is ±0.3mm.

3. The high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels according to claim 1, characterized in that, The composition and particle size of each powder in the coating are as follows: Marble: CaCO3≥98%, 40 mesh; Fluorite: CaF2≥96%, 40 mesh; Barium carbonate: BaCO3≥80%, 40 mesh; Quartz sand: SiO2≥99%, 40 mesh; Titanium dioxide: TiO2≥98%, 40 mesh; Zircon sand: ZrO2≥99%, 40 mesh; Rare earth ferrosilicon: RE≥30%, Si≥45%, 60 mesh; Ferromanganese: Mn≥75%, 80 mesh; Reduced iron powder: Fe≥98%, 80 mesh; Soda ash: Na2CO3≥99.2%, 200 mesh.

4. A method for preparing a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels, characterized in that, The method is used to implement the high-strength and tough welding electrode for welding high-pressure hydrogen storage pressure vessels as described in any one of claims 1-3, and includes the following steps: After annealing and heat treatment, the core wire is drawn with reduced diameter, then leveled and cut to form the core. The core contains the following components by mass fraction: C: 0.04%~0.08%; Si: 0.4%~0.6%; Mn: 1.4%~1.6%; Ni: 1.3%~1.8%; Cr: 0.1%~0.15%; Mo: 0.1%~0.2%; Ti: 0.04%~0.08%; B: 0.004%~0.007%; S≤0.005%; P≤0.008%; with the balance being Fe. The powdered medicinal materials are mixed together, and the components of the medicinal materials, by mass fraction, are: marble: 27%~35%; fluorite: 13%~18%; barium carbonate: 7%~9%; quartz sand: 4%~7%; titanium dioxide: 3%~5%; zircon sand: 2%~3%; rare earth ferrosilicon: 3%~5%; ferromanganese: 4%~6%; reduced iron powder: 13%~18%; soda ash: 1%~2%. Water glass is added to the mixed drug coating powder, and after mixing evenly, a drug coating material is formed. The prepared coating material is placed into the electrode coating machine so that the coating material is evenly adhered and wrapped on the surface of the electrode core to form a wet electrode. Wet welding electrodes are dried to form high-strength and tough welding electrodes for welding high-pressure hydrogen storage pressure vessels.

5. The method for preparing a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels according to claim 4, characterized in that, The annealing process of the core wire rod is controlled at 690±10℃×2h, and the single compression ratio range of the core wire rod drawing process is 9%~13%.

6. The method for preparing a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels according to claim 4, characterized in that, When wet mixing the drug coating powder, potassium sodium water glass with a modulus M of 3.1 and a Baumé degree (20℃) of 38~40ºBé is used.

7. The method for preparing a high-strength and high-toughness welding electrode for welding high-pressure hydrogen storage pressure vessels according to claim 4, characterized in that, When drying wet welding electrodes, a segmented drying method is adopted. After the wet welding electrodes are naturally dried at room temperature for 8 hours, they are dried using a process of 150℃×2h→300℃×2h→450℃×2h.

Citation Information

Patent Citations

  • Low-hydrogen basic electrode for 25Cr2Ni4MoV alloy steel welding

    CN101890594A