A waterproof breathable membrane and a preparation method thereof and a composite fabric comprising the same

Through the mixing of polyolefin raw materials and solvents and the biaxial stretching process, a waterproof and breathable membrane with uniform pore size and excellent penetration is prepared, which solves the problems of insufficient mechanical strength and environmental pollution of waterproof and breathable membranes in the existing technology, and achieves high performance, Low-cost waterproof and breathable membrane production.

CN118085386BActive Publication Date: 2024-10-11QINGDAO ZHONGKEHUALIAN ADVANCED MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410222282.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-10-11
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

Existing waterproof and breathable membranes have shortcomings in terms of waterproofing, breathability and mechanical strength. They are especially difficult to combine with knitted fabrics, and traditional processes have problems with environmental pollution and high costs.

Method used

Polyolefin raw materials are mixed with solvent white oil, antioxidants and elastomers are added, and microporous membranes are prepared through biaxial stretching and extraction processes, and then expanded, stretched, and heat-set to form a waterproof membrane with uniform pore size and excellent penetration. Breathable membrane.

Benefits of technology

It improves the elongation at break, puncture resistance and waterproof performance of the waterproof and breathable membrane, reduces costs, realizes an environmentally friendly and controllable production process, and is suitable for a variety of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118085386B_ABST
    Figure CN118085386B_ABST
Patent Text Reader

Abstract

The present invention provides a waterproof breathable membrane, a preparation method thereof, and a composite fabric comprising the same. The preparation method of the waterproof breathable membrane comprises: first mixing a polyolefin raw material with a solvent to obtain a premixed gel; second mixing an elastomer with a solvent, and then third mixing with the premixed gel to obtain a mixed gel; melt-extruding the mixed gel to obtain an initial gel membrane, then initially stretching it on a biaxial stretching machine, and then extracting it with an extractant to obtain an initial microporous membrane; bulking and stretching the initial microporous membrane, and then heat-setting and rapid high-temperature treatment in sequence. The waterproof breathable membrane is obtained by the preparation method. The composite fabric consists of an inner fabric and an outer fabric, and the waterproof breathable membrane provided by the present invention that is composited between the inner fabric and the outer fabric. The preparation method provided by the present invention is conducive to industrial promotion and use, and the obtained product has excellent waterproof and breathable properties and higher tensile strength and elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof materials, and in particular relates to a waterproof breathable membrane and a preparation method thereof, and a composite fabric comprising the same. Background Art

[0002] Waterproof breathable membrane is a functional membrane material that is both water-resistant and moisture-permeable. It can be combined with fiber fabrics to produce functional textiles with unique protection and comfort, and has a wide range of applications. With the improvement of people's living standards, the popularity of outdoor sports has also increased significantly, and outdoor sports have higher and higher requirements for functional textiles (such as jackets) that are both waterproof, breathable, warm, and have sufficient mechanical strength.

[0003] The waterproof and breathable membranes used in special clothing such as assault jackets and protective clothing are mostly made of PTFE and PU. PTFE is a fluorine-containing material and there is a possibility of environmental pollution. The European Union has issued restrictive regulations that will gradually restrict the application of fluorine-containing materials in the next 10 years. Conventional preparation methods for PU waterproof and breathable membranes include traditional processes such as cast film and blown film, and new processes such as electrospinning. The PE membrane produced by traditional processes has a large output and a low price, but due to technical conditions, the air permeability of the membrane is extremely poor. The new process PU membrane has good air permeability, but the output is low and the cost is high.

[0004] Casual wear, commuting wear, underwear, wearable devices, etc. in daily life are used frequently and for a long time, and they need to be waterproof and breathable. These clothes usually use knitted fabrics, which have good elasticity. The waterproof and breathable membranes made of conventional polyolefin materials are limited by their low elongation and are difficult to compound with knitted fabrics. They cannot meet normal use. Therefore, it is necessary to improve the elongation at break and puncture resistance of the material.

[0005] Patent CN117164995A discloses a polypropylene waterproof breathable membrane and its production process, which uses 70-90 parts of polypropylene as the main material, adds 15-25 parts of modified nano-silicon dioxide and additives such as regulators, plasticizers, and antioxidants, and then extrudes the membrane in a twin-screw extruder, first stretches it longitudinally and then stretches it transversely to obtain a polypropylene waterproof breathable membrane. The waterproof breathable membrane produced by this process has poor surface pore uniformity, poor air permeability, and low moisture permeability, which cannot meet people's daily needs.

[0006] Safe and environmentally friendly expanded PE / PP waterproof and breathable membrane is a new topic. It is expected to completely replace EPTFE and PU waterproof and breathable membranes in the future, and achieve adjustable pores, thickness, and surface of PE / PP waterproof and breathable membranes. It has great potential in the fields of medical treatment, clothing, electronic equipment, packaging, etc. Especially in the field of clothing, the environmental protection, biocompatibility, durability, and comfort of waterproof and breathable membranes are particularly important.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The object of the present invention is to provide a waterproof breathable membrane and a preparation method thereof and a composite fabric comprising the same, so as to solve the above-mentioned problems.

[0009] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:

[0010] The present invention provides a method for preparing a waterproof breathable membrane, comprising the following steps:

[0011] S1: mixing the polyolefin raw material and the solvent white oil to obtain a premixed gel for standby use;

[0012] The polyolefin raw material includes one or more of LLDPE, LDPE, HDPE, UHMWPE or PP; preferably, the polyolefin raw material is UHMWPE, and the molecular weight of the UHMWPE is 400,000-2,000,000;

[0013] The first mixing also includes adding 0.05-1% of the mass of the polyolefin raw material antioxidant; the antioxidant is selected from one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, pentaerythritol tetrakis(di-T-butyl hydroxyhydrocinnamate), antioxidant 1010, tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate pentaerythritol ester, tetrakis-(dibutyl hydroxyhydrocinnamate)pentaerythritol ester, tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)pentaerythritol ester), and antioxidant 168.

[0014] S2: performing a second mixing of the elastomer and the solvent white oil, and then performing a third mixing with the premixed gel obtained in S1 to obtain a mixed gel;

[0015] The elastomer includes one or more of thermoplastic elastomer (POE), EPDM, SBS, and EPR obtained by in-situ polymerization of ethylene and octene using a metallocene catalyst; preferably, the elastomer is a thermoplastic elastomer obtained by in-situ polymerization of ethylene and octene using a metallocene catalyst; further preferably, the added amount of the elastomer is 0.5-5% of the mass of the polyolefin raw material.

[0016] Optionally, the added amount of the elastomer may be any value between 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5% and 5% of the mass of the polyolefin raw material.

[0017] S3: melt-extrude the mixed gel obtained in S2 to obtain an initial gel membrane, then perform initial stretching on a biaxial stretching machine, and then extract with dichloromethane as an extractant to obtain an initial microporous membrane; preferably, the extraction further includes ultrasonic-assisted extraction;

[0018] The melt extrusion comprises: setting the screw temperature of the twin-screw extruder to 140°C-240°C, the melt pipe temperature to 190°C-230°C, and the die head temperature to 180°C-220°C, adding the mixed gel into the twin-screw extruder through a peristaltic pump for melt extrusion;

[0019] Optionally, the screw temperature of the twin-screw extruder may be any value between 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C and 240°C, the melt pipe temperature may be any value between 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C and 230°C, and the die temperature may be any value between 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C and 220°C;

[0020] The initial stretching includes room temperature stretching and temperature-raising stretching;

[0021] Preferably, the stretching ratio of the room temperature stretching is 1-2 times, and the stretching rate is 5-20 mm / s;

[0022] Further preferably, the stretching temperature of the temperature-increasing stretching is 60-100° C., the stretching multiple is 1-5 times, and the stretching rate is 5-20 mm / s.

[0023] Optionally, the stretching ratio of the room temperature stretching can be any value between 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2, and the stretching rate can be any value between 5 mm / s, 6 mm / s, 7 mm / s, 8 mm / s, 9 mm / s, 10 mm / s, 11 mm / s, 12 mm / s, 13 mm / s, 14 mm / s, 15 mm / s, 16 mm / s, 17 mm / s, 18 mm / s, 19 mm / s and 20 mm / s;

[0024] The stretching temperature of the temperature-increasing stretching can be any value between 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C and 100°C, the stretching ratio can be any value between 1 time, 1.5 times, 2 times, 2.5 times, 3 times, 3.5 times, 4 times, 4.5 times and 5 times, and the stretching rate can be any value between 5mm / s, 6mm / s, 7mm / s, 8mm / s, 9mm / s, 10mm / s, 11mm / s, 12mm / s, 13mm / s, 14mm / s, 15mm / s, 16mm / s, 17mm / s, 18mm / s, 19mm / s and 20mm / s.

[0025] The initial stretching is carried out in steps with obvious advantages. During the room temperature stretching process, due to the small stretching multiple, under the action of tensile stress, the chips undergo plastic deformation, the molecular chains are pulled out from the crystal region, and the spherulites gradually evolve into extended chain crystals. During the subsequent temperature increase stretching, the chain segments and molecular chains undergo changes, adjustments and rearrangements to release the internal stress. At the same time, the presence of white oil is conducive to the transmission of force and promotes the growth of the number of fibers, forming a uniformly distributed fiber network structure and orderly arrangement of the chips, so that the pore size distribution of the formed microporous membrane is more uniform and controllable, effectively improving its performance.

[0026] S4: The initial microporous membrane in S3 is expanded and stretched, and then heat-set and rapidly treated at high temperature in sequence to obtain the waterproof and breathable membrane.

[0027] The stretching temperature of the bulking stretching is 90-140°C, and the stretching ratio is 1-9 times;

[0028] Optionally, the stretching temperature of the bulking stretching can be any value between 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C and 140°C, and the stretching ratio can be any value between 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5 and 9 times;

[0029] The heat setting temperature is 90-130°C; optionally, the heat setting temperature can be any value between 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C and 130°C;

[0030] The rapid high temperature treatment comprises: using hot air with a temperature of 80-130° C. to blow for 1-10 seconds.

[0031] Optionally, the temperature of the rapid high temperature treatment can be any value between 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C and 130°C, and the purge time can be any value between 1s, 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s and 10s.

[0032] Rapid high-temperature treatment can make the internal fibers of the expanded and stretched waterproof and breathable membrane adhere to each other, reduce the material stratification phenomenon, and improve the waterproof performance and rubbing resistance of the waterproof and breathable membrane.

[0033] The present invention uses a polymer with good compatibility and cooperates with an original stretching process to improve the elongation at break and puncture resistance of the waterproof breathable membrane on the basis of ensuring porosity, uniform pore size and high moisture permeability. At the same time, the waterproof breathable membrane prepared by the method of thermally induced phase separation has controllable pore size and excellent permeability. In the present invention, the initial gel film can be subjected to initial stretching, and the white oil plays a role of speed increase and lubrication during the initial stretching process, which is conducive to the transmission of force to promote the growth of the number of fibers, form a fiber mesh structure, and make the wafers arranged in order. At the same time, the solvent is used as a porogen to form an original pore structure after extraction, and the pore size is uniform and fine. Bidirectional synchronous stretching is performed again, and the original pore structure is stretched and reorganized to obtain a waterproof breathable membrane with high porosity, controllable pore size and excellent permeability. Due to the existence of the topological structure between molecules, the fibrous crystal structure is refined and recrystallized to obtain a more uniform and fine microporous structure. At the same time, the oriented crystallization behavior existing in the stretching process significantly improves the tensile strength of the waterproof breathable membrane.

[0034] The waterproof and breathable membrane provided by the invention is prepared by the preparation method.

[0035] The present invention also provides a composite fabric, which is composed of an inner fabric, an outer fabric, and a waterproof and breathable membrane composited between the inner fabric and the outer fabric;

[0036] The waterproof and breathable membrane is prepared by the preparation method;

[0037] The inner layer fabric is one or more of woven fabrics, knitted fabrics, nonwoven fabrics and electrospun membranes obtained by pure spinning, blending, blended yarn or blended fibers of the fabric raw materials;

[0038] The outer layer fabric is one or more of woven fabrics, knitted fabrics, nonwoven fabrics and electrospun membranes obtained by pure spinning, blending, blended yarn or blended fibers of the fabric raw materials;

[0039] The raw materials of the fabric include one or more of cotton, linen, acetate, viscose, mulberry silk, polyester, nylon, aramid, spandex, polypropylene, chlorofiber, acrylic, wool, rabbit hair, camel hair, mohair, yak hair, metal fiber, and conductive fiber.

[0040] Preferably, the compounding includes hot melt adhesive powder dot coating compounding, hot melt adhesive slurry dot compounding, hot melt adhesive powder sprinkling compounding, hot melt adhesive double dot compounding, polyurethane spraying compounding, and polyurethane rolling compounding.

[0041] Beneficial effects of the present invention:

[0042] The preparation method provided by the present invention has simple and controllable conditions, cheap and easily available raw materials, good process repeatability, environmentally friendly and energy-saving process, and the obtained waterproof and breathable membrane has excellent comprehensive performance and high production capacity, which is conducive to industrial promotion and use.

[0043] The waterproof and breathable membrane provided by the present invention has uniform pore size, excellent mechanical properties, good hand feel, and rub resistance. It has excellent softness and can adapt to various complex shapes and surface structures. It also has low cost, large production capacity, and good application scenarios. It is more widely used in outdoor sports, medical dressings, military industry, construction, packaging, daily chemical industry and other industries.

[0044] The composite fabric made using the waterproof and breathable membrane provided by the present invention has higher mechanical properties than conventional fabrics and has excellent waterproof and breathable properties. The composite process is simple and has wide applicability, especially suitable for industries such as daily clothing, wearable devices and special clothing. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0046] Figure 1 A scanning electron microscope image of the initial gel film provided in Example 1;

[0047] Figure 2 This is a scanning electron microscope image of the initial microporous membrane provided in Example 1;

[0048] Figure 3 This is a scanning electron microscope image of the waterproof breathable membrane provided in Example 1. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0050] Example 1

[0051] The method for preparing a waterproof breathable membrane according to the present invention specifically comprises the following steps:

[0052] S1: Weigh 30 parts by weight of UHMWPE with a molecular weight of 750,000 and 50 parts by weight of white oil, stir and mix them evenly to obtain a polyolefin premixed gel;

[0053] S2: Weigh 1% of the mass of UHMWPE elastomer POE, 0.6% of the mass of UHMWPE antioxidant 1010, and 0.3% of the mass of UHMWPE antioxidant 168, and then heat and stir to mix evenly in 20 parts by mass of white oil at a heating temperature of 85°C. After being evenly mixed, stir and mix with the polyolefin premixed gel obtained in S1 to obtain a mixed gel;

[0054] S3: The mixed gel obtained in S2 was added to a twin-screw extruder through a peristaltic pump. The screw temperature was set to 180°C, the melt pipe temperature was 220°C, and the die temperature was 210°C. The initial gel film was extruded and then cooled at 35°C to form. The surface scanning electron microscope image is shown in FIG. Figure 1 As shown;

[0055] S4: the initial gel film obtained in S3 was cut into 12*12 cm film blocks, and initially stretched on a biaxial stretching machine, first at room temperature, with a stretching ratio of 1.3 times and a stretching rate of 5 mm / s, and then stretched at elevated temperature, with the temperature set to 85°C, the stretching ratio to 2 times and the stretching rate to 10 mm / s;

[0056] S5: The initial microporous membrane is extracted with dichloromethane after the initial stretching, and the scanning electron microscope image thereof is as follows: Figure 2 As shown, the film is then expanded and stretched, the stretching temperature is set to 120°C, the stretching ratio is 4 times, the heat setting temperature is 123°C, and the film is quickly blown with hot air at 130°C for 5s to obtain a waterproof and breathable film. The scanning electron microscope image is shown in Figure 3 shown.

[0057] pass Figure 1-Figure 3It can be seen that the appearance of the product film at each stage is uniform and maintains a certain shape. After being extruded by a twin-screw extruder, UHMWPE is linked to each other to form a spatial network structure, and the spatial pores are filled with white oil medium, which plays a role in speeding up lubrication. Figure 1 In the electron microscope image, after removing the white oil, the initial gel film has obvious pores and a cross-linked structure. Since the polymer compounds that make up the network have a certain degree of flexibility, the initial gel film has stretchability. Figure 2 It is a microporous membrane with uniform pore structure on the surface and nanometer-level pore diameter. During the room temperature stretching process, under the action of tensile stress, the crystal undergoes plastic deformation, the molecular chain is pulled out from the crystal area, and the spherulite gradually evolves into extended chain crystals; during the subsequent temperature-raising stretching, the chain segments and molecular chains undergo abnormal movement, adjustment and rearrangement, so that the internal stress is released, the fiber mesh structure is evenly distributed, and the crystals are arranged in an orderly manner, so that the pore size distribution of the microporous membrane formed subsequently is uniform, effectively improving its performance. Figure 3 The expanded waterproof breathable membrane provided by the present invention presents a fiber network multi-level expanded structure. Special expanded stretching promotes the growth of fibrils around the fibril connection nodes, generates a regularly staggered snowflake-shaped spatial structure, and obtains a waterproof breathable material with negative Poisson's ratio expanded pores. Rapid high-temperature treatment enhances the bonding force at the fibril connection points, releases internal stress, and reduces material stratification.

[0058] Example 2

[0059] The difference from Example 1 is that the amount of the elastomer POE in S2 is 3% of the mass of UHMWPE.

[0060] Example 3

[0061] The difference from Example 1 is that the amount of the elastomer POE in S2 is 5% of the mass of UHMWPE.

[0062] Example 4

[0063] The difference from Example 1 is that the polyolefin raw material used in S1 is PP with a molecular weight of 1 million, and the temperature of heating and stretching in S4 is 140°C.

[0064] Example 5

[0065] The difference from Example 1 is that the polyolefin raw material used in S1 is a blend of UHMWPE with a molecular weight of 400,000 and HDPE with a molecular weight of 160,000 in a mass ratio of 67:33.

[0066] Example 6

[0067] The difference from Example 1 is that the polyolefin raw material used in S1 is a blend of UHMWPE with a molecular weight of 400,000 and PP with a molecular weight of 1,000,000 in a mass ratio of 67:33.

[0068] Example 7

[0069] The waterproof breathable membrane prepared in Example 1 was compounded with the outer polyester fabric and the inner viscose fabric by double-point hot melt adhesive to prepare a waterproof breathable membrane composite fabric.

[0070] Comparative Example 1

[0071] The difference from Example 1 is that there is no initial stretching in step S4, that is, it does not include room temperature stretching and temperature-elevated stretching, and the membrane block is directly extracted with dichloromethane to obtain an initial microporous membrane, which is then expanded and stretched with a stretching ratio of 8 times.

[0072] Comparative Example 2

[0073] The raw materials were weighed as the first component according to the amounts of steps S1 and S2 in Example 1, mixed with the second component calcium carbonate powder in a ratio of 50:50, mixed evenly in a high-speed mixer, and then extruded into granules in a twin-screw extruder at 210° C., and then extruded into a sheet in a single-screw extruder and biaxially stretched at a stretching ratio of 9 times to obtain a microporous membrane.

[0074] Comparative Example 1

[0075] The difference from the embodiment is that no elastomer is added to S2.

[0076] Comparative Example 2

[0077] A commercially available PTFE waterproof and breathable membrane was selected.

[0078] Comparative Example 3

[0079] The conventional dry method is used to prepare the PE waterproof breathable membrane, which specifically includes:

[0080] 70 parts by weight of polyethylene with a molecular weight of 400,000, 30 parts by weight of calcium carbonate and 0.5 parts of an antioxidant are mixed evenly in a high-speed mixer, then extruded into granules at 190°C in a twin-screw extruder, and then extruded into sheets in a single-screw extruder and biaxially stretched with a stretching ratio of 6 times to obtain a microporous membrane.

[0081] The performance tests were conducted on the films or fabrics provided in the embodiments, control examples and comparative examples, and the results are shown in Table 1 below:

[0082] Table 1 Material performance test results

[0083]

[0084] By comparing Example 1 with Control Example 1, it can be seen that in Control Example 1, the initial gel film is directly extracted and then expanded and stretched without initial stretching. Although the waterproof and breathable membrane obtained has relatively good air permeability and large porosity, it is stretched and reshaped on the basis of defects, so it has poor uniformity and even worse mechanical properties, which is not conducive to wide application.

[0085] It can be seen from Table 1 that the waterproof breathable membrane prepared by the method adopted in the embodiment of the present invention, and the composite fabric prepared therefrom, show more excellent comprehensive performance, and the waterproofness, breathability, and mechanical properties are all at a high level, which is more conducive to its wide industrial use.

[0086] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A method for preparing a waterproof breathable membrane, characterized in that: The steps include: S1: mixing the polyolefin raw material and the solvent to obtain a premixed gel for standby use; S2: performing a second mixing of the elastomer and the solvent, and then performing a third mixing with the premixed gel obtained in S1 to obtain a mixed gel; S3: melt-extrude the mixed gel obtained in S2 to obtain an initial gel membrane, then perform initial stretching on a biaxial stretching machine, and then extract with an extractant to obtain an initial microporous membrane; S4: the initial microporous membrane in S3 is subjected to bulking and stretching, and then subjected to heat setting and rapid high-temperature treatment in sequence to obtain the waterproof and breathable membrane; The initial stretching includes room temperature stretching and temperature-elevated stretching; the stretching multiple of the room temperature stretching is 1-2 times, and the stretching rate is 5-20 mm / s; the stretching temperature of the temperature-elevated stretching is 60-100°C, the stretching multiple is 1-5 times, and the stretching rate is 5-20 mm / s; The rapid high temperature treatment comprises: using hot air with a temperature of 80-130° C. to blow for 1-10 seconds.

2. The preparation method according to claim 1, characterized in that: The step S1 satisfies one or more of the following conditions: a. The polyolefin raw material includes one or more of LLDPE, LDPE, HDPE, UHMWPE or PP; b. The solvent is white oil; c. The first mixing further includes adding 0.05-1% of the mass of the polyolefin raw material antioxidant.

3. The preparation method according to claim 2, characterized in that: The step S1 also satisfies one or more of the following conditions: d. The polyolefin raw material is UHMWPE, and the molecular weight of the UHMWPE is 400,000-2,000,000; e. The antioxidant is selected from one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, pentaerythritol tetrakis(di-T-butyl hydroxyhydrocinnamate), antioxidant 1010, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, pentaerythritol tetrakis-(dibutyl hydroxyhydrocinnamate), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate), and antioxidant 168.

4. The preparation method according to claim 1, characterized in that: The step S2 satisfies one or more of the following conditions: f. The elastomer comprises one or more of ethylene and octene in situ polymerized thermoplastic elastomer (POE), EPDM, SBS, and EPR using a metallocene catalyst; g. The solvent is white oil; h. The amount of the elastomer added is 0.5-5% of the mass of the polyolefin raw material.

5. The preparation method according to claim 1, characterized in that: The step S3 satisfies one or more of the following conditions: i. The melt extrusion comprises: setting the screw temperature of the twin-screw extruder to 140°C-240°C, the melt pipe temperature to 190°C-230°C, the die temperature to 180°C-220°C, and adding the mixed gel to the twin-screw extruder through a peristaltic pump for melt extrusion; j. The extractant is dichloromethane.

6. The preparation method according to claim 1, characterized in that: The stretching temperature of the bulking stretching is 90-140° C., and the stretching multiple is 1-9 times.

7. A waterproof breathable membrane, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.

8. A composite fabric, characterized in that: The composite fabric is composed of an inner fabric, an outer fabric, and a waterproof and breathable membrane composited between the inner fabric and the outer fabric; The waterproof breathable membrane is prepared by the preparation method according to any one of claims 1 to 6; The inner layer fabric is one or more of woven fabrics, knitted fabrics, nonwoven fabrics and electrospun membranes obtained by pure spinning, blending, blended yarn or blended fibers of the fabric raw materials; The outer layer fabric is one or more of woven fabrics, knitted fabrics, nonwoven fabrics and electrospun membranes obtained by pure spinning, blending, blended yarn or blended fibers of the fabric raw materials; The raw materials of the fabric include one or more of cotton, linen, acetate, viscose, mulberry silk, polyester, nylon, aramid, spandex, polypropylene, chloroprene, acrylic, wool, rabbit hair, camel hair, mohair, yak hair, metal fiber, and conductive fiber.

9. The composite fabric according to claim 8, characterized in that: The compounding includes hot melt adhesive powder dot coating compounding, hot melt adhesive slurry dot compounding, hot melt adhesive powder sprinkling compounding, hot melt adhesive double dot compounding, polyurethane spraying compounding, and polyurethane rolling compounding.