A wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing

By evaluating the denitrification efficiency and resistance changes of the catalyst at different temperatures, the low-load deactivation capacity of the catalyst was determined. Through high-temperature recovery technology, the problem of the denitrification system being unable to operate due to catalyst blockage caused by ammonium bisulfate was solved, realizing safe operation of the catalyst under low load and saving on retrofit investment.

CN118098413BActive Publication Date: 2026-11-17SUZHOU XIRE ENERGY SAVING ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410154974.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2026-11-17
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively address the problem of denitrification systems being unable to operate under low-load conditions due to catalyst blockage caused by ammonium bisulfate (ABS), and the assessment methods do not consider the impact of actual flue gas conditions, leading to increased retrofit investment and operational risks.

Method used

By changing the inlet flue gas temperature of the SCR denitrification unit, the denitrification efficiency and resistance changes of the catalyst under different temperature conditions are evaluated, the low-load deactivation capacity of the catalyst is determined, and the catalyst activity is restored by rapidly increasing the load, obtaining high-temperature recovery characteristic parameters to guide the safe operation of the catalyst at low temperatures.

Benefits of technology

Without upgrading the equipment to increase its temperature, the catalyst's ability to operate under low loads is explored, providing key parameters to enable normal operation of coal-fired units under deep peak shaving, reducing investment in upgrades and workload in operation and maintenance, and improving the catalyst's adaptability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118098413B_ABST
    Figure CN118098413B_ABST
Patent Text Reader

Abstract

This invention discloses a wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing. The method includes the following steps: changing the inlet flue gas temperature of the SCR denitrification unit; evaluating the change in catalyst low-load ABS deactivation capacity based on the changes in denitrification efficiency and catalyst resistance under different flue gas temperature conditions; exploring the catalyst's low-load operating capacity while ensuring safe operation; and evaluating the minimum allowable operating temperature of the catalyst under designed sulfur content. After the catalyst low-load deactivation evaluation is completed, the catalyst activity is restored by rapidly increasing the inlet flue gas temperature, obtaining the characteristic parameters of catalyst high-temperature recovery. This invention explores the catalyst's low-load operating performance, adjusts the coal feed, and enables normal operation of the SCR denitrification system under deep peak-shaving conditions in coal-fired power units without equipment temperature-increasing modifications. This saves on modification investment, reduces equipment operation and maintenance workload, and provides technical support for the flexible modification of coal-fired power units.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst performance evaluation technology, specifically relating to a wide-temperature operation evaluation method for catalysts with low load, moderate deactivation, and high-temperature recovery based on field testing. Background Technology

[0002] Currently, the peak-shaving lower limit for most gas-fired power units in China is 30%–40% BMCR, with some coal-fired power units even reaching as low as 15% BMCR, corresponding to temperatures below 270℃. Most coal-fired power units currently employ SCR flue gas denitrification systems based on vanadium-titanium catalysts. The low inlet flue gas temperature under low-load conditions, preventing the denitrification system from operating, is a significant factor limiting deep peak-shaving. Theoretical research indicates that under low load conditions, SO3 molecules exceeding the saturation partial pressure within the catalyst micropores will undergo capillary condensation, generating liquid ammonium bisulfate (ABS) within the micropores. This process is determined by flue gas temperature and SO3 concentration, and is also influenced by factors such as cross-sectional flue gas temperature distribution and dust concentration. Between the catalyst's lowest continuous ammonia injection temperature (MOT temperature) and the ABS precipitation dew point temperature, capillary condensation causes micropore ABS blockage, leading to a continued temperature decrease. When approaching the ABS precipitation dew point temperature, blockage after macroscopic ABS precipitation must be considered. In recent years, the impact of ABS precipitation under low load conditions on catalyst performance and lifespan has received widespread attention from domestic research institutions.

[0003] To achieve low-load operation of denitrification catalysts, the current mainstream method uses laboratory catalyst evaluation and catalyst manufacturer design parameters, which have a relatively high safety margin. However, their use is limited under actual flue gas conditions, making it difficult to put the catalyst into safe and reliable operation under low load, or requiring a large investment of human, material and financial resources for efficiency improvement.

[0004] Chinese invention patent, publication number CN109433011A, discloses a method for expanding the low-load commissioning potential of SCR denitrification based on the catalyst's ammonium bisulfate poisoning recovery characteristics. This method eliminates the need for on-site equipment temperature upgrades, fully utilizes the catalyst's inherent low-load adaptability to achieve wide-load commissioning of the denitrification system, reduces modification investment, avoids downtime affecting unit power generation, and lowers the risk of equipment modifications impacting normal unit operation. However, this patent is based on catalyst performance evaluation under laboratory conditions and does not consider the influence of factors such as sulfur content changes and ash accumulation under actual flue gas conditions, thus limiting the scope of the evaluation data.

[0005] Chinese invention patent, publication number CN112717690A, discloses a method for SCR denitrification operation under deep peak shaving conditions in coal-fired power units. During deep peak shaving, the method improves the catalyst's applicability by evaluating the catalyst's MOT temperature and explores its low-load operation capability. However, this patent does not consider the catalyst's moderate deactivation and high-temperature recovery capabilities under actual flue gas conditions.

[0006] Among the various methods currently disclosed for putting SCR denitrification catalysts into operation during low load or deep peak shaving, apart from using laboratory conditions to evaluate MOT temperature, the main approach is to use temperature-raising modifications such as flue gas bypass to meet the catalyst's operating conditions. However, there is currently no control method that utilizes conventional catalysts' low-load moderate deactivation and high-temperature recovery to further explore the catalyst's low-temperature operating capability and improve its operational adaptability. Summary of the Invention

[0007] To address the technical problems existing in the prior art, the present invention aims to provide a wide-temperature operation evaluation method for catalysts under low-load moderate deactivation and high-temperature recovery based on field testing. This method tests and evaluates the changes in various performance parameters before and after the first layer of catalyst, and evaluates the performance changes of the catalyst based on the changes in the amount of denitrification catalyst under low-load moderate deactivation and high-temperature recovery, thereby guiding the wide-temperature operation of denitrification units.

[0008] To achieve the above objectives and technical effects, the technical solution adopted by this invention is as follows:

[0009] A wide-temperature operation evaluation method for catalysts undergoing moderate deactivation and high-temperature recovery under low load based on field testing includes the following steps:

[0010] The inlet flue gas temperature of the SCR denitrification unit is changed. The changes in denitrification efficiency and catalyst resistance under different flue gas temperature conditions are used to evaluate the changes in the catalyst's low-load ABS deactivation capacity. Under the premise of ensuring the safe operation of the unit, the catalyst's low-load operating capacity is explored. The minimum allowable operating temperature of the catalyst under the designed sulfur content is evaluated. The low-load deactivation evaluation of the catalyst is then completed.

[0011] After the catalyst deactivation assessment at low load is completed, the catalyst activity is restored by rapidly increasing the load to raise the inlet flue gas temperature. Characteristic parameters of high-temperature catalyst recovery are obtained, providing key parameters for low-temperature catalyst operation and guiding the safe operation of the catalyst at low temperatures.

[0012] Furthermore, the method includes the following steps:

[0013] 1) First, conduct a low-load assessment of the denitrification unit and arrange the measuring points, then proceed to Phase 1:

[0014] Based on the sulfur content of the coal fed into the furnace and the design parameters of the catalyst performance, the minimum continuous ammonia injection temperature T0 of the catalyst, the design efficiency of a single catalyst layer η0, the design catalyst resistance ΔP0, and the minimum operating temperature attenuation coefficients k1 and k2 are designed.

[0015] In the first stage, the NOx concentration in the flue gas at the inlet of the first catalyst layer of the SCR reactor and the NOx concentration in the flue gas at the outlet of the first catalyst layer are tested. At the initial moment, the SO3 concentration in the flue gas at the outlet of the first catalyst layer and the static pressure difference ΔP1 between the inlet and outlet of the first catalyst layer are measured. The denitrification efficiency η1 at the initial moment is calculated and verified. If the deactivation assessment conditions are met, the second stage of deactivation operation assessment is carried out.

[0016] 2) Stage 2: Reduce the operating temperature from temperature T0 to temperature T1. After stabilization, conduct Stage 2 testing to obtain the static pressure difference ΔP2 between the inlet and outlet flue gas of the first catalyst layer. Calculate the denitrification efficiency η2 at the initial moment and perform verification calculation. If the deactivation assessment conditions are met, continue to conduct Stage 3 deactivation operation assessment.

[0017] 3) Stage 3: Reduce the operating temperature from temperature T1 to temperature T2. After stabilization, conduct Stage 3 testing to obtain the static pressure difference ΔP3 of the flue gas at the inlet and outlet of the first catalyst layer. Calculate the denitrification efficiency η3 at the initial moment and perform verification calculation. If the deactivation assessment conditions are met, continue to conduct Stage 4 deactivation operation assessment.

[0018] 4) And so on, until the nth stage, when temperature T is reached. n-1 After the temperature stabilizes, if one of the deactivation assessment conditions is not met, the minimum operating temperature T is reached. n-1 This is the lowest permissible operating temperature under the current operating conditions of the catalyst, marking the end of the low-load deactivation operation assessment of the catalyst;

[0019] After the catalyst low-load deactivation operation assessment is completed, the flue gas temperature is increased to T according to the catalyst low-load requirements and the unit load increase rate. N After running for a time S at this temperature, a test is performed. If the following conditions are met simultaneously after the test: η N ≥(0.97~1.0)*η0、△P N If the temperature rise is less than or equal to (1.0~1.1)*△P0, then the high-temperature recovery is complete, and the recovery temperature rise R=T is recorded. N -T0, recovery time S.

[0020] Furthermore, in step 1), the inactivation assessment conditions include:

[0021] a) η1≥k1*η0, k1=0.3~0.6;

[0022] b)△P1≤k2*△P0, k2=1.2~1.5;

[0023] Only when both inactivation assessment conditions a) and b) are met simultaneously can the second stage of inactivation operation assessment proceed.

[0024] Furthermore, in step 2), the inactivation assessment conditions include:

[0025] c) η2≥k1*η0, k1=0.3~0.6;

[0026] d)△P2≤k2*△P0, k2=1.2~1.5;

[0027] If either c) or d) is not met, the evaluation test ends. Only if both c) and d) are met can the third stage of inactivation operation evaluation continue.

[0028] Furthermore, in step 3), the inactivation assessment conditions include:

[0029] e) η3≥k1*η0, k1=0.3~0.6;

[0030] f)△P3≤k2*△P0, k2=1.2~1.5;

[0031] If either e) or f) is not met, the evaluation test ends. Only if both e) and f) are met can the next stage of inactivation operation evaluation be carried out.

[0032] Furthermore, in step 2), the temperature T1 is 5 to 10°C lower than the temperature T0.

[0033] Furthermore, in step 3), the temperature T2 is 5 to 10°C lower than the temperature T1.

[0034] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0035] This invention discloses a wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing. The method involves changing the inlet flue gas temperature of the denitrification unit and evaluating the changes in denitrification efficiency and catalyst resistance under different flue gas temperatures to assess the catalyst's low-load ABS deactivation capacity. This method aims to explore the catalyst's low-load operating capacity while ensuring safe unit operation. The minimum allowable operating temperature of the catalyst under sulfur content is determined using tests conducted under actual flue gas conditions, marking the end of the low-load deactivation evaluation. After the low-load deactivation evaluation, the catalyst activity is restored by rapidly increasing the inlet flue gas temperature. The catalyst's activity recovery capacity is then evaluated based on field testing to obtain the catalyst's high-temperature recovery capacity. The recovered characteristic parameters (recovery temperature rise and recovery time) provide key parameters for low-temperature catalyst operation, guiding the safe operation of the catalyst at low temperatures. This invention is based on the close correlation between the MOT temperature of the SCR catalyst and flue gas conditions, and the recoverability of the catalyst's performance after ammonium bisulfate poisoning. By exploring the low-load operation performance of the catalyst and adjusting the coal fed into the furnace, the SCR denitrification system can be put into normal operation under deep peak-shaving conditions in coal-fired power units without equipment temperature-raising modifications. This saves on modification investment, reduces the workload of subsequent equipment operation and maintenance, provides technical support for the flexible modification of coal-fired power units, and is of great significance for further promoting the formation of wide-temperature operation control technology based on moderate catalyst deactivation and high-temperature recovery. Attached Figure Description

[0036] Figure 1 This is a flowchart of the present invention;

[0037] Figure 2 This is a schematic diagram of the low-load evaluation measurement point layout of the denitrification device of the present invention. Detailed Implementation

[0038] The present invention will now be described in detail so that its advantages and features can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.

[0039] The following provides a brief overview of one or more aspects to offer a basic understanding of them. This overview is not an exhaustive summary of all conceived aspects, nor is it intended to identify key or decisive elements of all aspects, nor to define the scope of any or all aspects. Its sole purpose is to present some concepts of one or more aspects in a simplified form to prepare for the more detailed descriptions that follow.

[0040] like Figure 1-2 As shown, a wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing includes the following steps:

[0041] 1) First, conduct a low-load assessment of the denitrification unit and arrange the measurement points; enter the first stage: select the design feed coal sulfur content of the denitrification system according to the actual situation of the unit, select the initial temperature T0 according to the design feed coal sulfur content and catalyst performance design parameters, T0 is generally the minimum continuous ammonia injection temperature (MOT temperature) of the catalyst, and select the design catalyst single-layer efficiency η0, the design catalyst resistance ΔP0 and the minimum operating temperature decay coefficient k.

[0042] In the first stage, the NOx concentration (C) in the inlet flue gas of the first catalyst layer 1 of the SCR reactor was tested. NOx,in,1 NOx concentration in the flue gas at the outlet of the first catalyst layer 1 (C) NOx,out,1 The SO3 concentration (C) in the flue gas exiting the first catalyst layer 1 was measured at the initial moment. SO3,out,1 Given the static pressure difference ΔP1 between the inlet and outlet flue gas of the first catalyst layer 1, calculate the initial denitrification efficiency η1. η1 is stable when the flue gas remains constant. The calculation is verified under the following conditions:

[0043] a) η1≥k1*η0, k1=0.3~0.6;

[0044] b) △P1≤k2*△P0, k2=1.2~1.5, △P0 is the resistance of the first catalyst layer;

[0045] If both deactivation assessment conditions a) and b) are met, then proceed to the second stage of deactivation operation assessment;

[0046] 2) Stage 2: After decreasing the initial temperature T1 by approximately 5–10°C to reach temperature T2, and stabilizing for approximately 15–30 minutes, stage 2 testing is conducted. In stage 2, the NOx concentration (C2) in the flue gas at the inlet of catalyst 1 in the SCR reactor is measured. NOx,in,2 NOx concentration in the flue gas at the outlet of the first catalyst layer 1 (C) NOx,out,2 The SO3 concentration (C) in the flue gas exiting the first catalyst layer 1 was measured at the initial moment. SO3,out,2 Given the static pressure difference ΔP2 between the inlet and outlet flue gas of the first catalyst layer 1, calculate the initial denitrification efficiency η2. η2 will decrease from η1. The calculation is verified under the following conditions:

[0047] c) η2≥k1*η0, k1=0.3~0.6;

[0048] d)△P2≤k2*△P0, k2=1.2~1.5;

[0049] If either c) or d) fails to meet the inactivation assessment condition, the assessment experiment ends. If both c) and d) meet the inactivation assessment conditions, the third stage of inactivation operation assessment continues.

[0050] 3) Stage 3: After decreasing the temperature by approximately 5–10°C from T2 to reach T3, and stabilizing for approximately 15–30 minutes, stage 3 testing is conducted. In stage 3, the NOx concentration (Cg) in the flue gas at the inlet of the first catalyst layer of the SCR reactor is measured. NOx,in,3 NOx concentration in the flue gas at the outlet of the first catalyst layer 1 (C) NOx,out,3 The SO3 concentration (C) in the flue gas exiting the first catalyst layer 1 was measured at the initial moment. SO3,out,3 Given the static pressure difference ΔP3 between the inlet and outlet flue gas of the first catalyst layer 1, calculate the initial denitrification efficiency η3. η3 will decrease from η2. The calculation is verified under the following conditions:

[0051] e) η3≥k1*η0, k1=0.3~0.6;

[0052] f)△P3≤k2*△P0, k2=1.2~1.5;

[0053] If either e) or f) fails to meet the inactivation assessment condition, the assessment test ends. If both e) and f) meet the inactivation assessment conditions, the next stage of inactivation operation assessment continues.

[0054] 4) And so on, until the nth stage, when temperature T is reached. n After the temperature stabilizes, if one of the deactivation assessment conditions is not met, the minimum operating temperature T is reached. n This is the lowest permissible operating temperature under the current operating conditions of the catalyst, marking the end of the low-load deactivation phase of the catalyst;

[0055] After the catalyst deactivation assessment at low load is completed, in accordance with the low load requirements, the catalyst activity must be restored by rapidly increasing the load to raise the inlet flue gas temperature of the denitrification unit. The flue gas temperature should be increased to T according to the unit's load increase rate. N T N Generally, the temperature is 15-25°C higher than T0. After running for a time (S) at this temperature, the test is performed. If the following conditions are met simultaneously after the test: η N ≥(0.97~1.0)*η0、△P N If the temperature rise is less than or equal to (1.0~1.1)*△P0, then the high-temperature recovery is complete, and the recovery temperature rise is recorded as R=T. N -T0, recovery time S, generally decreases as the R value increases.

[0056] Therefore, the characteristic operating parameters for catalyst deactivation under low load and high temperature recovery include: the minimum allowable operating temperature T under the current operating conditions of the catalyst. n The high-temperature recovery time S and the catalyst recovery temperature rise R. In actual catalyst operation, if the minimum operating temperature of the catalyst is higher than T... nIf the temperature rises above R and the recovery time is greater than S after low-load operation, the catalyst activity can be effectively activated, with little impact on the catalyst life and virtually no risk of low-temperature deactivation. Under low load, the SO3 concentration and NH3 in the flue gas pose little risk of ABS blockage in the catalyst channels.

[0057] In this invention, the formula for calculating the denitrification efficiency is:

[0058] η=(C NOx,in -C NOx,out )*100 / C NOx,in

[0059] in:

[0060] η represents the denitrification efficiency, in percent.

[0061] C NOx,in The NOx concentration in the catalyst inlet flue gas is converted to standard conditions, dry basis, 6% O2, in mg / m³. 3 ;

[0062] C NOx,out The NOx concentration in the catalyst outlet flue gas is converted to standard conditions, dry basis, and 6% O2, in mg / m³. 3 .

[0063] C NH3,out The concentration of NH3 in the catalyst outlet flue gas is calculated to standard conditions, on a dry basis, under 6% O2, in mg / m³. 3 .

[0064] △P is the static pressure difference between the inlet and outlet flue gas of the first catalyst layer, in Pa.

[0065] C SO3,out The concentration of SO3 in the catalyst outlet flue gas is converted to standard conditions, dry basis, and 6% O2, in mg / m³. 3 .

[0066] Example 1

[0067] Taking a 660MW wall-mounted opposed-flow combustion boiler as an example, this invention illustrates the evaluation process of a wide-temperature operation evaluation method based on field testing for catalyst low-load moderate deactivation and high-temperature recovery. Figure 1-2 As shown:

[0068] 1) According to the actual characteristics of the unit, the sulfur content of the coal fed into the furnace is 1.2%, the denitration device has a total of 3 layers of catalysts arranged sequentially from top to bottom, the designed single-layer efficiency of the catalyst η0=75%, the resistance of the first-layer catalyst ΔP0=125Pa, the designed minimum continuous ammonia injection temperature is 295°C, and the 4th group of modules on side A is selected as the evaluation object. According to the existing operation requirements, k1=0.45, k2=1.5, in the first stage of deactivation evaluation, the minimum continuous ammonia injection temperature T1=T0=295°C is selected, and after stabilizing for 30 minutes, the NOx concentration value (C in the flue gas at the inlet of the first layer catalyst 1 of the SCR reactor is tested NOx,in,1 ), the NOx concentration value (C in the flue gas at the outlet of the first layer catalyst 1 NOx,out,1 ), at the initial moment, measure the SO3 concentration value (C in the flue gas at the outlet of the first layer catalyst 1 SO3,out,1 ) and the static pressure difference ΔP1 of the flue gas at the inlet and outlet of the first layer catalyst 1, calculate the denitration efficiency η1 at the initial moment, and perform verification calculation, as shown in Table 1:

[0069] Table 1

[0070] project unit numerical values <![CDATA[C NOx,in,1 ]]> <![CDATA[mg / m 3 ]]> 425 <![CDATA[C NOx,out,1 ]]> <![CDATA[mg / m 3 ]]> 110 <![CDATA[C SO3,out,1 ]]> <![CDATA[mg / m 3 ]]> 12.5 <![CDATA[η1]]> % 74.1 <![CDATA[△P1]]> Pa 118

[0071] It can be seen from Table 1 that η1=74.1%, k1*η0=33.75%, η1>k1*η0, condition a) is satisfied; ΔP1=118Pa, k2*ΔP0=187.5Pa, ΔP1<k2*ΔP0, condition b) is also satisfied, then the deactivation operation evaluation of the second stage is continued.

[0072] 2) Decrease by 10°C on the basis of the initial temperature T1 to reach T2=285°C, after stabilizing for 30 minutes, test the NOx concentration value (C in the flue gas at the inlet of the first layer catalyst 1 of the SCR reactor NOx,in,2 ), the NOx concentration value (C in the flue gas at the outlet of the first layer catalyst 1 NOx,out,2 ), at the initial moment, measure the SO3 concentration value (C in the flue gas at the outlet of the first layer catalyst 1 SO3,out,2 ) and the static pressure difference ΔP2 of the flue gas at the inlet and outlet of the first layer catalyst 1, calculate the denitration efficiency η2 at the initial moment, and perform verification calculation, as shown in Table 2:

[0073] Table 2

[0074] project unit numerical values <![CDATA[C NOx,in,2 ]]> <![CDATA[mg / m 3 ]]> 436 <![CDATA[C NOx,out,2 ]]> <![CDATA[mg / m 3 ]]> 178 <![CDATA[C SO3,out,2 ]]> <![CDATA[mg / m 3 ]]> 9.5 <![CDATA[η2]]> % 59.2 <![CDATA[△P2]]> Pa 141

[0075] It can be seen from Table 2 that η2=59.2%, k1*η0=33.75%, η2>k1*η0, condition a) is satisfied; ΔP2=141Pa, k2*ΔP0=187.5Pa, ΔP2<k2*ΔP0, condition b) is also satisfied, then the deactivation operation evaluation of the third stage is continued.

[0076] 3) Decrease by 10°C on the basis of temperature T2 to reach temperature T3=275°C, and after stabilizing for 30 min, test the NOx concentration value (C of the flue gas at the inlet of the first layer catalyst 1 of the SCR reactor NOx,in,3 ), the NOx concentration value (C of the flue gas at the outlet of the first layer catalyst 1 NOx,out,3 ), measure the SO3 concentration value (C of the flue gas at the outlet of the first layer catalyst 1 at the initial moment SO3,out,3 ) and the static pressure difference ΔP3 of the flue gas at the inlet and outlet of the first layer catalyst 1, calculate the denitration efficiency η3 at the initial moment, and perform verification calculation, as shown in Table 3:

[0077] Table 3

[0078] project unit numerical values <![CDATA[C NOx,in,3 ]]> <![CDATA[mg / m 3 ]]> 453 <![CDATA[C NOx,out,3 ]]> <![CDATA[mg / m 3 ]]> 246 <![CDATA[C SO3,out,3 ]]> <![CDATA[mg / m 3 ]]> 3.2 <![CDATA[η3]]> % 45.7 <![CDATA[△P3]]> Pa 162

[0079] It can be seen from Table 3 that η3=45.7%, k1*η0=33.75%, η3>k1*η0, condition a) is satisfied; ΔP3=162Pa, k2*ΔP0=187.5Pa, ΔP3<k2*ΔP0, condition b) is also satisfied, then proceed to the deactivation operation assessment of the 4th stage.

[0080] 4) Decrease by 6°C on the basis of temperature T3 to reach temperature T4=269°C, and after stabilizing for 30 min, test the NOx concentration value (C of the flue gas at the inlet of the first layer catalyst 1 of the SCR reactor NOx,in,4 ), the NOx concentration value (C of the flue gas at the outlet of the first layer catalyst 1 NOx,out,4 ), measure the SO3 concentration value (C of the flue gas at the outlet of the first layer catalyst 1 at the initial moment SO3,out,4 ) and the static pressure difference ΔP4 of the flue gas at the inlet and outlet of the first layer catalyst 1, calculate the denitration efficiency η4 at the initial moment, and perform verification calculation, as shown in Table 4:

[0081] Table 4

[0082] project unit numerical values <![CDATA[C NOx,in,4 ]]> <![CDATA[mg / m 3 ]]> 445 <![CDATA[C NOx,out,4 ]]> <![CDATA[mg / m 3 ]]> 304 <![CDATA[C SO3,out,4 ]]> <![CDATA[mg / m 3 ]]> 3.2 <![CDATA[η4]]> % 31.7 <![CDATA[△P4]]> Pa 175

[0083] It can be seen from Table 4 that η4=31.7%, k1*η0=33.75%, η4<k1*η0, condition a) is not satisfied, ΔP4=175Pa, k2*ΔP0=187.5Pa, ΔP4<k2*ΔP0, condition b) is satisfied. Since the denitration efficiency has dropped to the minimum lower limit at this time, the catalyst deactivation assessment is completed, and T4=269°C is the minimum operating temperature of the catalyst.

[0084] 5) After the catalyst low-load deactivation assessment is completed, in accordance with the catalyst low-load requirements, it is necessary to increase the inlet flue gas temperature by rapidly increasing the load to restore the catalyst activity, and in accordance with the unit load increase rate, increase the flue gas temperature to T N=310℃, and after running at this temperature for S=3h, the NOx concentration (C) in the inlet flue gas of the first catalyst layer 1 of the SCR reactor was measured. NOx,in,5 NOx concentration in the flue gas at the outlet of the first catalyst layer 1 (C) NOx,out,5 The concentration of SO3 in the flue gas at the outlet of the first catalyst layer 1 was measured (C). SO3,out,5 The initial denitrification efficiency η5 was calculated based on the static pressure difference ΔP5 between the inlet and outlet flue gas of the first catalyst layer 1 and the first catalyst layer 1. The calculation was then verified, as shown in Table 5.

[0085] Table 5

[0086] project unit numerical values <![CDATA[C NOx,in,5 ]]> <![CDATA[mg / m 3 ]]> 445 <![CDATA[C NOx,out,5 ]]> <![CDATA[mg / m 3 ]]> 235 <![CDATA[C SO3,out,5 ]]> <![CDATA[mg / m 3 ]]> 6.8 <![CDATA[η5]]> % 47.2 <![CDATA[△P5]]> Pa 158

[0087] As shown in Table 5, η5 = 47.2% < η n =0.98*η0=73.5%, △P5=158Pa>1.05*△P0=131.25Pa, then the heating time needs to be extended at this temperature.

[0088] 5) After continuing to raise the temperature for 7.5 hours, continue testing the parameters and measure the NOx concentration (C) in the inlet flue gas of the first catalyst layer 1 in the SCR reactor. NOx,in,6 NOx concentration in the flue gas at the outlet of the first catalyst layer 1 (C) NOx,out,6 The concentration of SO3 in the flue gas at the outlet of the first catalyst layer 1 was measured (C). SO3,out,6 The initial denitrification efficiency η6 is calculated based on the static pressure difference ΔP6 between the inlet and outlet flue gas of the first catalyst layer 1 and the first catalyst layer 1. The calculation is then verified, as shown in Table 6.

[0089] Table 6

[0090] project unit numerical values <![CDATA[C NOx,in,6 ]]> <![CDATA[mg / m 3 ]]> 426 <![CDATA[C NOx,out,6 ]]> <![CDATA[mg / m 3 ]]> 109 <![CDATA[C SO3,out,6 ]]> <![CDATA[mg / m 3 ]]> 13.8 <![CDATA[η6]]> % 74.4 <![CDATA[△P6]]> Pa 128

[0091] As shown in Table 6, η6 = 74.4% > η n =0.98*η0=73.5%, △P6=128Pa<1.05*△P0=131.25Pa, the high temperature recovery of the catalyst is completed, and the catalyst activity is fully restored.

[0092] As can be seen from the above, the catalyst's performance evaluation based on low-temperature moderate deactivation and high-temperature recovery shows that, under the current condition of 1.2% sulfur content in the coal fed into the furnace, the minimum operating ammonia injection temperature is approximately 269℃, and the high-temperature recovery temperature and time are 310℃ and 7.5h, respectively.

[0093] Based on the final evaluation of wide-temperature operation with low load, moderate deactivation, and high-temperature recovery, under the current condition of 1.2% sulfur content in the coal fed into the furnace, the minimum operating ammonia injection temperature is approximately 269℃, and the high-temperature recovery temperature and time are 310℃ and 7.5h, respectively. This is significantly lower than the minimum ammonia injection operating temperature designed for the catalyst, which can greatly increase the operating time of the catalyst during deep peak shaving and the initial stage of grid connection. Under the premise of ensuring catalyst safety, the limitations of low-temperature operation of the catalyst are reduced, and the economic and safe operation capability of the denitrification unit is improved.

[0094] Any parts or structures not specifically described in this invention can be made using existing technologies or products, and will not be elaborated upon here.

[0095] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A method for wide temperature operation evaluation of catalyst low load moderate deactivation high temperature recovery based on field test, characterized in that, Includes the following steps: The inlet flue gas temperature of the SCR denitrification unit is changed. The changes in denitrification efficiency and catalyst resistance under different flue gas temperature conditions are used to evaluate the changes in the catalyst's low-load ABS deactivation capacity. Under the premise of ensuring the safe operation of the unit, the catalyst's low-load operating capacity is explored. The minimum allowable operating temperature of the catalyst under the designed sulfur content is evaluated. The low-load deactivation evaluation of the catalyst is then completed. After the catalyst deactivation assessment under low load is completed, the catalyst activity is restored by rapidly increasing the inlet flue gas temperature by increasing the load. Characteristic parameters of high-temperature catalyst recovery are obtained, providing key parameters for low-temperature catalyst operation and guiding the safe operation of the catalyst at low temperatures. 1) First, conduct a low-load assessment of the denitrification unit and arrange the measuring points, then proceed to Phase 1: Based on the sulfur content of the coal fed into the furnace and the design parameters of the catalyst performance, the minimum continuous ammonia injection temperature T0 of the catalyst, the design efficiency of a single catalyst layer η0, the design catalyst resistance ΔP0, and the minimum operating temperature attenuation coefficients k1 and k2 are designed. In the first stage, the NOx concentration in the flue gas at the inlet of the first catalyst layer of the SCR reactor and the NOx concentration in the flue gas at the outlet of the first catalyst layer are tested. At the initial moment, the SO3 concentration in the flue gas at the outlet of the first catalyst layer and the static pressure difference ΔP1 between the inlet and outlet of the first catalyst layer are measured. The denitrification efficiency η1 at the initial moment is calculated and verified. If the deactivation assessment conditions are met, the second stage of deactivation operation assessment is carried out. 2) Stage 2: Reduce the operating temperature from temperature T0 to temperature T1. After stabilization, conduct Stage 2 testing to obtain the static pressure difference ΔP2 between the inlet and outlet flue gas of the first catalyst layer. Calculate the denitrification efficiency η2 at the initial moment and perform verification calculation. If the deactivation assessment conditions are met, continue to conduct Stage 3 deactivation operation assessment. 3) Stage 3: Reduce the operating temperature from temperature T1 to temperature T2. After stabilization, conduct Stage 3 testing to obtain the static pressure difference ΔP3 of the flue gas at the inlet and outlet of the first catalyst layer. Calculate the denitrification efficiency η3 at the initial moment and perform verification calculation. If the deactivation assessment conditions are met, continue to conduct Stage 4 deactivation operation assessment. 4) In turn, to the nth stage, the temperature T n-1 , after the temperature is stable, it does not meet one of the deactivation evaluation conditions, and reaches the minimum operating temperature T n-1 , which is the minimum allowable operating temperature under the current operating conditions of the catalyst, and the catalyst low load deactivation operation evaluation ends; When the catalyst low load deactivation operation evaluation is over, the flue gas temperature is increased to T N at the required low load of the catalyst, at the unit load increase rate, after the operation time value S at this temperature, if the following conditions are met simultaneously after the test: η N ≥ (0.97~1.0)*η0, ΔP N ≤ (1.0~1.1)*△P0, then the high temperature recovery is over, and the recovery temperature rise R=T N -T0, recovery time S is recorded.

2. The method for catalyst wide temperature operation evaluation based on field test with low load moderate deactivation and high temperature recovery according to claim 1, characterized in that, In step 1), the inactivation assessment conditions include: a) η1≥k1*η0, k1=0.3~0.6; b) △P1≤k2*△P0, k2=1.2~1.5; Only when both inactivation assessment conditions a) and b) are met simultaneously can the second stage of inactivation operation assessment proceed.

3. The method for catalyst wide temperature operation evaluation based on field test with low load moderate deactivation and high temperature recovery according to claim 1, characterized in that, In step 2), the inactivation assessment conditions include: c) η2≥k1*η0, k1=0.3~0.6; d) △P2≤k2*△P0, k2=1.2~1.5; If either c) or d) is not met, the evaluation test ends. Only if both c) and d) are met can the third stage of inactivation operation evaluation continue.

4. The wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing as described in claim 1, characterized in that, In step 3), the inactivation assessment conditions include: e) η3≥k1*η0, k1=0.3~0.6; f) △P3≤k2*△P0, k2=1.2~1.5; If either e) or f) is not met, the evaluation test ends. Only if both e) and f) are met can the next stage of inactivation operation evaluation be carried out.

5. The wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing, as described in claim 1, is characterized in that... In step 2), the temperature T1 is 5~10℃ lower than the temperature T0.

6. The wide-temperature operation evaluation method for catalyst low-load moderate deactivation and high-temperature recovery based on field testing, as described in claim 1, is characterized in that... In step 3), the temperature T2 is 5~10℃ lower than the temperature T1.

Citation Information

Patent Citations

  • Method for widening SCR denitration low-load operation potential based on ammonium bisulfate poisoning recovery characteristics of catalyst

    CN109433011A

  • SCR denitration commissioning method under deep peak regulation working condition of coal-fired unit

    CN112717690A

  • Device and method for evaluating low-load operation adaptability of coal-fired flue gas denitration catalyst