A method for preparing leaching reagents for efficient in-situ leaching mining of low-grade uranium ore
By using the reflux reaction of tertiary amine, aqueous ethanol solution, potassium thiocyanate and hydrochloric acid in the preparation method, combined with a suitable diluent, the problems of low leaching efficiency and environmental pollution of low-grade uranium ore are solved, and a highly efficient and environmentally friendly uranium ore leaching reagent preparation is achieved, with a leaching rate as high as 98%.
Patent Information
- Application Number
- CN202211482585.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In existing technologies, hydrochloric acid and sulfuric acid are inefficient and cause serious environmental pollution when used for leaching low-grade uranium ore, making it difficult to effectively extract uranium resources.
A viscous liquid [R3NH][SCN] was prepared by reflux reaction of a tertiary amine, an aqueous ethanol solution, potassium thiocyanate, and hydrochloric acid in a reactor. A diluent was then added to prepare a leaching reagent. Trioctyldecyl tertiary amine N235 was preferred as the tertiary amine. By combining suitable reaction conditions and diluent types, the leaching efficiency was improved.
The prepared leaching reagent has a leaching rate of over 98%, is easy to produce on a large scale, has good industrial application value, and reduces environmental pollution.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrometallurgy, and particularly relates to a method for preparing a leaching reagent for efficient leaching mining of low-grade uranium ore. Background Technology
[0002] Uranium is generally considered a rare metal. Although it is abundant in the Earth's crust, far more so than mercury, bismuth, and silver, its discovery was delayed considerably due to the difficulty of extraction. As the last naturally occurring radioactive element in the periodic table, metallic uranium plays a vital role in our world. For example, the heat released during its radioactive decay, along with its neighbor thorium, provides a significant amount of energy to the Earth's core and continuously or unpredictably alters the thinner layers of the Earth's crust.
[0003] The discovery of uranium fission completely changed the definition of "total conflict" in warfare. All the properties of metallic uranium originate from its unique nuclear characteristics. However, some other characteristics of uranium are not entirely determined by its unique nucleus and may also be related to the electrons orbiting the nucleus. These extraordinary properties are little known, and therefore possess significant scientific value.
[0004] Currently, the main processes for uranium extraction and recovery are leaching and extraction. Leaching methods primarily involve hydrochloric acid leaching and sulfuric acid leaching, while extraction methods mainly include solvent extraction, precipitation, ion exchange, and liquid membrane extraction. The use of hydrochloric acid or sulfuric acid leaching often leads to significant environmental problems, and conventional extraction methods also have various drawbacks. Therefore, developing a green, economical, and environmentally friendly leaching reagent is of paramount importance. Summary of the Invention
[0005] This invention addresses the exploration of leaching reagents for low-grade uranium ore. Ordinary leaching agents are difficult to use for leaching low-grade uranium ore. While hydrochloric acid and sulfuric acid have leaching effects, the leaching rates are low, and leaching with hydrochloric acid or sulfuric acid causes significant environmental problems. This invention provides a method for preparing a leaching reagent for the efficient leaching of low-grade uranium ore.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore includes the following steps:
[0008] In a reaction vessel, tertiary amine, aqueous ethanol solution, potassium thiocyanate, and hydrochloric acid are added respectively, and the mixture is stirred and refluxed at room temperature. Then, excess solvent is removed by rotary evaporation to obtain a viscous liquid [R3NH][SCN]. A diluent is then added according to the amount of [R3NH][SCN] to obtain a reagent for leaching low-grade uranium ore.
[0009] Furthermore, the mass fractions of the tertiary amine, aqueous ethanol solution, potassium thiocyanate, and hydrochloric acid are 2-12 parts, 6-20 parts, 4-15 parts, and 1-6 parts, respectively.
[0010] Furthermore, the tertiary amine is one or more of trioctylamine TOA, triisooctylamine TiOA, and trioctyldecyl tertiary amine N235.
[0011] Furthermore, the trioctyldecyl tertiary amine has three branches attached to N, and these three branches have the same structure, with eight to ten carbons, resulting in excellent leaching performance. Considering economic benefits, the preferred tertiary amine is trioctyldecyl tertiary amine N235.
[0012] Furthermore, the reflux reaction time is 8-36 hours.
[0013] Furthermore, based on the fluidity and mass transfer efficiency of the solution during the reaction, the volume ratio of water to ethanol in the ethanol-water solution is determined, and the preferred volume ratio of water to ethanol is 1:0.5-5.
[0014] Furthermore, the amount and method of adding hydrochloric acid are determined based on the degree of temperature change during the reaction process, with the preferred method of adding hydrochloric acid being dropwise in batches.
[0015] Furthermore, the type of diluent is determined based on the solubility of the leaching reagent [R3NH][HSO4], and the diluent is preferably water, ethanol, or an aqueous solution of ethanol.
[0016] Furthermore, the amount of the diluent added is 8-25 times the mass of [R3NH][HSO4].
[0017] The advantages of this invention compared to the prior art are:
[0018] This invention addresses the exploration of leaching reagents for low-grade uranium ore. Ordinary leaching agents are difficult to use for leaching low-grade uranium ore. While hydrochloric acid and sulfuric acid have leaching effects, the leaching rates are low, and leaching with hydrochloric acid or sulfuric acid causes significant environmental problems. This invention provides a method for preparing a highly efficient leaching reagent for low-grade uranium ore. This uranium ore leaching reagent has the advantages of simple preparation, ease of large-scale production, and high leaching efficiency, with a elution rate exceeding 98%, making it highly valuable for industrial applications. Detailed Implementation
[0019] The following specific embodiments further illustrate the content of the present invention, but should not be construed as limiting the present invention. Any modifications or substitutions made to the methods, steps, or conditions of the present invention without departing from the spirit and substance of the present invention should be covered within the scope of the claims of the present invention. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can all be obtained commercially.
[0020] Example 1: Preparation and Performance Study of Uranium Leaching Reagent
[0021] 1) Preparation of Leaching Agent
[0022] In a reaction vessel, add 4 parts of N235, 10 parts of a mixed solution of ethanol and water, 6 parts of potassium thiocyanate, and 2 parts of hydrochloric acid. Stir and reflux at room temperature for 24 hours. Then, remove excess solvent by rotary evaporation to obtain a viscous liquid [N235H][SCN]. Then, add 20 times the mass of ethanol according to the amount of [N235H][SCN] to obtain the leaching reagent for low-grade uranium.
[0023] (ii) Study on the leaching properties of uranium
[0024] Five times the volume of uranium leaching reagent was added to a low-grade uranium ore sample, and the mixture was allowed to stand for 12 hours. The aqueous phase was then analyzed, and the uranium content in the aqueous phase was found to be 0.099 g / L. The leaching rate was calculated to be 99.0%.
[0025] Example 2: Preparation and Performance Study of Uranium Leaching Reagent
[0026] 1) Preparation of Leaching Agent
[0027] In a reaction vessel, add 8 parts of TOA, 16 parts of a mixed solution of ethanol and water, 10 parts of potassium thiocyanate, and 4 parts of hydrochloric acid. Stir and reflux at room temperature for 24 hours. Then, remove excess solvent by rotary evaporation to obtain a viscous liquid [TOAH][SCN]. Then, add 20 times the mass of ethanol according to the amount of [TOAH][SCN] to obtain the leaching reagent for low-grade uranium.
[0028] (ii) Study on the leaching properties of uranium
[0029] Five times the volume of uranium leaching reagent was added to a low-grade uranium ore sample, and the mixture was allowed to stand for 12 hours. The aqueous phase was then analyzed, and the uranium content in the aqueous phase was found to be 0.098 g / L. The leaching rate was calculated to be 98.0%.
[0030] Example 3: Preparation and Performance Study of Uranium Leaching Reagent
[0031] 1) Preparation of Leaching Agent
[0032] In a reaction vessel, add 10 parts TiOA, 20 parts ethanol and water mixture, 12 parts potassium thiocyanate and 5 parts hydrochloric acid, stir and reflux at room temperature for 24 hours, then remove excess solvent by rotary evaporation to obtain a viscous liquid [TiOAH][SCN]. Then, add 20 times the mass of ethanol according to the amount of [TiOAH][SCN] to obtain the leaching reagent for low-grade uranium.
[0033] (ii) Study on the leaching properties of uranium
[0034] Five times the volume of uranium leaching reagent was added to a low-grade uranium ore sample, and the mixture was allowed to stand for 12 hours. The aqueous phase was then analyzed, and the uranium content in the aqueous phase was found to be 0.099 g / L. The leaching rate was calculated to be 99.0%.
[0035] Example 4: Treatment method for uranium leaching mining
[0036] (1) Leaching: 5% [N235H][SCN] leaching reagent is injected into the ore layer through the injection well, and then the uranium-containing leaching reagent is extracted through the pumping well;
[0037] (2) Pretreatment: The uranium-containing solution is filtered;
[0038] (3) Adsorption: Then, using uranium-oriented adsorption resin as adsorbent, the uranium-containing solution was subjected to column adsorption. The diameter-to-height ratio of the packing column was 1:5, and the operating temperature was 20℃.
[0039] (4) Desorption: The obtained uranium-loaded saturated resin is then eluted with a desorbent, which is a mixed solution of sodium chloride and sodium bicarbonate, with a concentration of 2% for both sodium chloride and sodium bicarbonate; the desorption volume is 4 BV, the operating temperature is 20°C, and the eluent after passing through the column is collected.
[0040] (5) Obtaining the product: The uranium-containing leaching solution is acidified with hydrochloric acid to pH 4.5 for 1 hour; sodium hydroxide is added to precipitate for 1 hour, the precipitate is aged for 12 hours, and the precipitate filtration pressure is 0.3 MPa.
[0041] The uranium recovery rate is over 85%.
[0042] The embodiments described above are merely preferred embodiments of the present invention, and not all feasible embodiments of the present invention. Any obvious modifications made by those skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore, characterized in that, The process includes the following steps: In a reaction vessel, a tertiary amine, an aqueous ethanol solution, potassium thiocyanate, and hydrochloric acid are added separately, and the mixture is stirred and refluxed at room temperature. Then, excess solvent is removed by rotary evaporation to obtain a viscous liquid [R3NH][SCN]. A diluent is then added according to the amount of [R3NH][SCN] to obtain a reagent for leaching low-grade uranium ore. The mass fractions of the tertiary amine, aqueous ethanol solution, potassium thiocyanate, and hydrochloric acid are 2-12 parts, 6-20 parts, 4-15 parts, and 1-6 parts, respectively. The tertiary amine is one or more of trioctylamine TOA, triisooctylamine TiOA, and trioctyldecyl tertiary amine N235.
2. The method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore as described in claim 1, characterized in that, The reflux reaction time is 8-36 h.
3. The method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore as described in claim 1, characterized in that, The volume ratio of water to ethanol in the ethanol-water solution is 1:0.5-5.
4. The method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore as described in claim 1, characterized in that, The preferred method for adding hydrochloric acid is to add it dropwise in batches.
5. The method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore as described in claim 1, characterized in that, The diluent is preferably water, ethanol, or an aqueous solution of ethanol.
6. The method for preparing a leaching reagent for efficient in-situ leaching mining of low-grade uranium ore as described in claim 1, characterized in that, The amount of the diluent added is 8-25 times the mass of [R3NH][HSO4].
Citation Information
Patent Citations
Recovery method of uranium using ionic liquid
JP2011107156A