A bimetallic catalyst, its preparation method, and its application in the catalytic preparation of ethanolamine from serine.

By using a biomass-based carbon-based solid acid-supported bimetallic catalyst, the problems of high pressure hazards and difficulty in catalyst separation in the preparation of ethanolamine in existing technologies have been solved, achieving highly selective decarboxylation of serine and providing an environmentally friendly and efficient preparation method.

CN118122341BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211530880.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2026-11-17
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

Existing technologies for preparing ethanolamine suffer from problems such as high-pressure reaction conditions being dangerous, difficulty in separating catalysts, and environmental unfriendliness, making it difficult to achieve highly selective decarboxylation of serine.

Method used

A biomass-based carbon-based solid acid-supported bimetallic catalyst was used to achieve the decarboxylation reaction of serine through the synergistic effect of the bimetallic sites composed of noble and non-noble metals and the support. This avoids the use of inorganic acids, simplifies the operation, and promotes the separation of the product from the aqueous phase.

Benefits of technology

The catalyst was developed to produce ethanolamine with high selectivity under mild conditions. It is easy to separate and recycle, environmentally friendly, and has high product yield and good catalytic activity stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003975880480000071
    Figure BDA0003975880480000071
  • Figure BDA0003975880480000081
    Figure BDA0003975880480000081
  • Figure BDA0003975880480000121
    Figure BDA0003975880480000121
Patent Text Reader

Abstract

This application discloses a bimetallic catalyst, its preparation method, and its application in the catalytic preparation of ethanolamine from serine. The method involves introducing hydrogen gas into a mixture containing serine, the catalyst, and water to initiate a decarboxylation reaction, yielding ethanolamine. The catalyst comprises a support and a bimetallic component loaded on the support, wherein the support is a biomass-based carbon-based solid acid. The bimetallic sites on the catalyst and the support work synergistically to achieve the decarboxylation of serine to ethanolamine. The reaction is simple, the catalyst is easily separable, environmentally friendly, and exhibits good cycle stability. This method and the catalyst have broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a bimetallic catalyst, its preparation method, and its application in the catalytic preparation of ethanolamine from serine, belonging to the field of chemical synthesis technology. Background Technology

[0002] Ethanolamine is an important fine organic chemical raw material and the most practically valuable amino alcohol. It possesses properties of both amines and alcohols, and is widely used in surfactants, petroleum additives, rubber plasticizers and foaming agents, as well as in gas purification, pharmaceuticals, and military applications (Chem.Eng.Process.2020,153,107930-107940). Methods for synthesizing ethanolamine include: chloroethanol ammonolysis, formaldehyde cyanohydrin catalytic hydrogenation, nitroethanol reduction, and ethylene oxide ammonolysis. The main route for producing ethanolamine involves the reaction of ethylene oxide with excess ammonia, using water or ammonia as a catalyst. This method requires high pressure to prevent ammonia vaporization at the reaction temperature. For safety reasons, ethylene oxide must be added to the ammonia solution; otherwise, it will cause explosive polymerization of ethylene oxide. In contrast, the decarboxylation reaction using the structural characteristics of serine to prepare ethanolamine has many advantages, such as milder reaction conditions and simpler experimental operation.

[0003] Serine, named after its origin in silkworm silk, is also known as β-hydroxyalanine. It is a neutral aliphatic hydroxyl-containing amino acid and a non-essential amino acid. Serine plays a role in cell membrane fabrication and processing, as well as in the synthesis of muscle tissue and the sheaths surrounding nerve cells. It can be obtained from natural proteins through methods such as protein hydrolysis. Its structural formula contains one hydroxyl group, one amino group, and one carboxyl group. Utilizing the characteristics of its structural functional groups, ethanolamine can be prepared through a decarboxylation reaction. Summary of the Invention

[0004] This application aims to provide a biomass carbon-based solid acid supported bimetallic heterogeneous catalyst for hydrogenating and removing the carboxyl group from serine to prepare ethanolamine.

[0005] According to the first aspect of this application, a method for preparing ethanolamine from serine is provided. The method utilizes a catalyst with bimetallic sites and a support that work synergistically to achieve serine decarboxylation and ethanolamine preparation. The method is simple to operate, the catalyst is easily separable, environmentally friendly, and exhibits good cycle stability. Using hydrogen as the hydrogen source, the method utilizes biomass-based carbon-based solid acid as the catalyst support to suppress deamination side reactions, prevent excessive protonation of the carboxyl group, slow down deoxygenation, and hinder decarbonylation, thereby achieving high selectivity for serine. Furthermore, the use of biomass-based carbon-based solid acid avoids the corrosion of equipment by inorganic acids and facilitates the separation of the product from the aqueous phase, demonstrating broad application prospects.

[0006] According to one aspect of this application, a bimetallic catalyst is provided, the bimetallic catalyst comprising a support and a bimetallic component supported on the support;

[0007] The bimetallic component is selected from noble metals and non-noble metals;

[0008] The precious metal is selected from at least one of Au, Pd, Pt, Rh, and Ru;

[0009] The non-precious metal is selected from at least one of Mo, Fe, Co, Ni, and Cu;

[0010] The carrier is a biomass carbon-based solid acid.

[0011] In the catalyst, the mass content of the noble metal is 0.2-15 wt%.

[0012] Optionally, the noble metal in the catalyst has a mass content of 1 to 8 wt%.

[0013] Optionally, in the catalyst, the mass content of the noble metal is any value or a range between 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, and 8wt%.

[0014] In the catalyst, the mass content of the non-precious metal is 5-50 wt%;

[0015] Optionally, the non-precious metal in the catalyst has a mass content of 10-30 wt%.

[0016] Optionally, in the catalyst, the mass content of the non-precious metal is any value among 10wt%, 20wt%, and 30wt%, or a range between any two.

[0017] The biomass carbon-based solid acid is obtained through the following steps:

[0018] 1) Carbonize biomass raw materials to obtain biomass-based carbon materials;

[0019] 2) The biomass-based carbon material obtained in 1) is mixed with an aqueous solution containing a sulfonating agent, reacted in a sealed container, and dried to obtain the biomass-based solid acid;

[0020] The biomass raw material is selected from at least one of starch, cellulose, chitin, corn cob powder, poplar powder, and birch powder;

[0021] The carbonization treatment temperature is 200–1000℃;

[0022] Optionally, the carbonization treatment temperature is 300–800°C;

[0023] Optionally, the carbonization temperature is any value among 300℃, 400℃, 500℃, 600℃, 700℃, and 800℃, or a range between any two.

[0024] The carbonization treatment time is 1 to 10 hours;

[0025] Optionally, the carbonization process takes 2 to 5 hours.

[0026] Optionally, the carbonization time is any value among 2h, 3h, 4h, and 5h, or a range between any two.

[0027] The sulfonating agent is selected from at least one of 98wt% concentrated sulfuric acid, p-toluenesulfonic acid, dodecylbenzenesulfonic acid, and aminosulfonic acid;

[0028] The mass ratio of the sulfonating agent to the biomass-based carbon material obtained in step 1) is 0.5 to 30;

[0029] Optionally, the mass ratio of the sulfonating agent to the biomass-based carbon material obtained in step 1) is any value from 0.5, 1, 5, 10, 15, 20, 25, 30 or any range between the two.

[0030] In the aqueous solution containing the sulfonating agent, the concentration of the sulfonating agent is 2.5 to 60 wt%.

[0031] Optionally, the concentration of the sulfonating agent is any value from 2.5wt%, 20wt%, 33wt%, 43wt%, 50wt%, 60wt%, or any range between both.

[0032] The reaction is a hydrothermal reaction;

[0033] The reaction temperature is 90–200°C;

[0034] Optionally, the reaction temperature is 150–180°C;

[0035] Optionally, the temperature of the reaction is any value of 150°C, 160°C, 170°C, 180°C, or a range between any two.

[0036] The reaction time is 0.5–15 h;

[0037] Optionally, the reaction time is 4 to 12 hours;

[0038] Optionally, the reaction time is any value among 4h, 8h, and 12h, or a range between any two.

[0039] The drying temperature is 50–120°C;

[0040] Optionally, the drying temperature is 90–110°C;

[0041] Optionally, the drying temperature is any value among 90°C, 100°C, and 110°C, or a range between any two.

[0042] The drying time is 8–72 hours;

[0043] Optionally, the drying time is 10 to 24 hours.

[0044] Optionally, the drying time is any value among 10h, 12h, 18h, and 24h, or a range between any two.

[0045] According to another aspect of this application, a method for preparing the above-mentioned bimetallic catalyst is provided, characterized in that,

[0046] Includes the following steps:

[0047] The support was immersed in an aqueous solution containing a bimetallic precursor, then dried, calcined, and reduced to obtain the bimetallic catalyst.

[0048] The bimetallic component precursor is selected from noble metal precursors and non-noble metal precursors;

[0049] The noble metal precursor is selected from at least one of chloroauric acid, palladium chloride, hexachloroplatinic acid, rhodium chloride, and ruthenium chloride;

[0050] The non-precious metal precursor is selected from at least one of ammonium molybdate, ferric nitrate, cobalt acetate, nickel nitrate, and copper chloride;

[0051] The impregnation is an equal-volume impregnation;

[0052] The drying temperature is 90–150°C;

[0053] Optionally, the drying temperature is 100–120°C;

[0054] Optionally, the drying temperature is any value among 100°C, 110°C, and 120°C, or a range between any two.

[0055] The drying time is 8–16 hours;

[0056] Optionally, the drying time is 10 to 12 hours;

[0057] Optionally, the drying time is any value among 10h, 11h, and 12h, or a range between any two.

[0058] The calcination temperature is 200–800℃;

[0059] Optionally, the calcination temperature is 400–600°C;

[0060] Optionally, the calcination temperature is any value among 400℃, 500℃, and 600℃, or a range between any two.

[0061] The calcination time is 2 to 10 hours;

[0062] Optionally, the calcination time is 2 to 8 hours;

[0063] Optionally, the calcination time is any value among 2h, 4h, 6h, and 8h, or a range between any two.

[0064] The reducing atmosphere is a hydrogen atmosphere;

[0065] The reduction temperature is 200–500°C;

[0066] Optionally, the reduction temperature is 300–450°C;

[0067] Optionally, the reduction temperature is any value among 300℃, 350℃, 400℃, and 450℃, or a range between any two.

[0068] The reduction time is 2–8 hours;

[0069] Optionally, the restoration time is 2 to 5 hours.

[0070] Optionally, the restoration time is any value among 2h, 3h, 4h, and 5h, or a range between any two.

[0071] Optionally, the catalyst is prepared by the following method:

[0072] The carbonization process of biomass raw materials involves mixing biomass-based carbon materials with a certain amount of sulfonating agent aqueous solution, followed by hydrothermal treatment, filtration and washing until neutral, and drying to obtain a carrier biomass carbon-based solid acid. The carrier is then impregnated in a solution containing a metal precursor, and the catalyst is obtained by stirring, settling, drying, calcining, and reducing.

[0073] Optionally, the specific conditions for stirring and mixing include:

[0074] The stirring speed is 500-1500 rpm, preferably 700-1000 rpm;

[0075] The stirring time is 0.2-2.5 hours, preferably 0.5-1 hour;

[0076] Optionally, the upper limit of the stirring speed is selected from 700 rpm, 800 rpm, 1000 rpm, 1200 rpm, and 1500 rpm; the lower limit is selected from 500 rpm, 700 rpm, 800 rpm, 1000 rpm, and 1200 rpm.

[0077] Optionally, the upper limit of the stirring time is selected from 0.5h, 0.8h, 1h, 1.5h, and 2.5h; and the lower limit is selected from 0.2h, 0.5h, 0.8h, 1h, and 1.5h.

[0078] Optionally, the specific conditions for stirring include:

[0079] The stirring speed is 500-1200 rpm, preferably 600-800 rpm;

[0080] The stirring time is 0.1-6 hours, preferably 0.5-4 hours;

[0081] The settling time is 12-48 hours, preferably 12-24 hours.

[0082] Optionally, the upper limit of the stirring speed is selected from 600 rpm, 800 rpm, 900 rpm, 1000 rpm, and 1200 rpm; the lower limit is selected from 500 rpm, 600 rpm, 800 rpm, 900 rpm, and 1000 rpm.

[0083] Optionally, the upper limit of the stirring time is selected from 0.5h, 1h, 1.5h, 4h, and 6h; and the lower limit is selected from 0.1h, 0.5h, 1h, 1.5h, and 4h.

[0084] Optionally, the upper limit of the settling time is selected from 16h, 24h, 30h, 36h, and 48h; and the lower limit is selected from 12h, 16h, 24h, 30h, and 36h.

[0085] According to another aspect of this application, a method for catalytically preparing ethanolamine from serine is provided, characterized in that...

[0086] Includes the following steps:

[0087] Hydrogen gas is introduced into a mixture containing serine, catalyst, and water to carry out a decarboxylation reaction, yielding ethanolamine.

[0088] The catalyst is selected from the bimetallic catalysts described above or the bimetallic catalysts prepared by the above preparation method.

[0089] The molar amount of the catalyst is 0.1% to 25% of the molar amount of the serine;

[0090] Optionally, the molar amount of the catalyst is any value from 0.1%, 0.5%, 1%, 5%, 10%, 15%, 20%, 25% of the molar amount of serine, or a range between any two.

[0091] The pressure of the hydrogen gas is 1–4 MPa;

[0092] Optionally, the pressure of the hydrogen gas is 2-3 MPa;

[0093] Optionally, the pressure of the hydrogen gas is any value among 2 MPa, 2.5 MPa, and 3 MPa, or a range between any two.

[0094] The temperature for the decarboxylation reaction is 150–260°C;

[0095] Optionally, the temperature of the decarboxylation reaction is 180–220°C;

[0096] Optionally, the temperature of the decarboxylation reaction is any value among 180°C, 190°C, 200°C, 210°C, and 220°C, or a range between any two.

[0097] The decarboxylation reaction takes 1–24 hours;

[0098] Optionally, the decarboxylation reaction takes 1 to 12 hours.

[0099] Optionally, the decarboxylation reaction time is any value among 1h, 2h, 4h, 6h, 8h, 10h, and 12h, or a range between any two.

[0100] In one specific embodiment, serine, catalyst and water are added to a reaction vessel, mixed, heated to 150-260°C, hydrogen partial pressure is 1.0-4.0 MPa, and reaction time is 1-24 h, serine is decarboxylated to produce glycine.

[0101] In one specific embodiment, this application provides a method for preparing a bimetallic catalyst and its application in the preparation of glycolic acid from serine. The method involves carbonizing a biomass raw material, mixing the resulting biomass-based carbon material with a certain amount of sulfonating agent aqueous solution, subjecting the mixture to hydrothermal treatment, filtering and washing until neutral, and drying to obtain a supported biomass carbon-based solid acid. The support is then impregnated in a solution containing a metal precursor to obtain the catalyst; wherein the support is a biomass carbon-based solid acid. The catalyst used in this method exhibits synergistic effects between the bimetallic sites and the support, enabling the decarboxylation of serine to prepare ethanolamine. The reaction is simple, the catalyst is easily separated, it is environmentally friendly, and it demonstrates good cycle stability. This method and the catalyst have broad application prospects.

[0102] This catalyst can decarboxylate serine to prepare ethanolamine. The catalyst is environmentally friendly, easy to separate from the system, and can maintain high catalytic activity after being recycled multiple times.

[0103] The beneficial effects that this application can produce include:

[0104] 1) The method for preparing ethanolamine by decarboxylation of serine provided in this application achieves decarboxylation of carboxylic acid group by the synergistic effect of the bimetallic site of the catalyst and the support, thereby obtaining glycolic acid from serine.

[0105] 2) The biomass carbon-based solid acid catalyst carrier used in this method helps to suppress the deamination side reaction during the reaction process, thereby achieving high selectivity for serine. At the same time, the use of biomass carbon-based solid acid avoids equipment corrosion and is more conducive to the separation of products from the aqueous phase, making it environmentally friendly.

[0106] 3) The catalyst in this application can still maintain good stability after being recycled five times, and the yield of the product remains above 60%. Detailed Implementation

[0107] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0108] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0109] In the embodiments of this application, the conversion rate and yield are calculated as follows:

[0110]

[0111]

[0112] Example 1

[0113] (1) The biomass raw material is placed in a tube furnace and carbonized at 300°C for 2 hours under a nitrogen atmosphere. The biomass raw material is corn cob powder. The obtained biomass-based carbon material is mixed with an aqueous sulfonating agent solution at 700 rpm for 0.5 hours. The sulfonating agent is 98 wt% concentrated sulfuric acid. The mass ratio of the sulfonating agent to the biomass-based carbon material is 5. The concentration of the sulfonating agent is 20 wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner and hydrothermally treated at 180°C for 4 hours. The solution is filtered, washed, and washed with deionized water until neutral. It is then dried at 90°C for 24 hours to obtain a biomass-based solid acid carrier.

[0114] (2) 0.1 g of support and 8 wt% of ruthenium chloride and 30 wt% of cobalt acetate were added to water with a saturated water absorption capacity of 0.1 g of support. After stirring at 800 rpm for 0.5 h, the mixture was allowed to stand at room temperature for 12 h and dried at 100 °C for 10 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 400 °C for 2 h and then reduced at 300 °C for 2 h under a hydrogen atmosphere to obtain a Ru-Co bimetallic catalyst.

[0115] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0116] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of ruthenium in the catalyst was 5% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 3.0 MPa of hydrogen gas was introduced. The temperature was raised to 180 °C, and the reaction was carried out at this temperature for 12 h. After the reaction, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 65%.

[0117] Example 2:

[0118] (1) The biomass raw material is placed in a tube furnace and carbonized at 800°C for 5 hours under a nitrogen atmosphere. The biomass raw material is starch. The obtained biomass-based carbon material is mixed with an aqueous sulfonating agent at 1000 rpm for 1 hour. The sulfonating agent is p-toluenesulfonic acid. The mass ratio of the sulfonating agent to the biomass-based carbon material is 30. The concentration of the sulfonating agent is 60 wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner and hydrothermally treated at 150°C for 10 hours. The solution is filtered, washed, and washed with deionized water until neutral. It is then dried at 110°C for 10 hours to obtain a biomass-based solid acid carrier.

[0119] (2) 0.1 g of support and 1 wt% palladium chloride and 10 wt% copper chloride were added to water with a saturated water absorption capacity of 0.1 g support. After stirring at 600 rpm for 4 h, the mixture was allowed to stand at room temperature for 24 h and dried at 120 °C for 12 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 600 °C for 8 h and then reduced at 200 °C for 8 h under a hydrogen atmosphere to obtain a Pd-Cu bimetallic catalyst.

[0120] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0121] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of palladium in the catalyst was 10% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 2.0 MPa of hydrogen gas was introduced. The temperature was raised to 220 °C, and the reaction was carried out at this temperature for 5 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 63%.

[0122] Example 3

[0123] (1) The biomass raw material is placed in a tube furnace and carbonized at 1000℃ for 1h under a nitrogen atmosphere, wherein: the biomass raw material is chitin; the obtained biomass-based carbon material is mixed with an aqueous sulfonating agent at 500rpm for 2.5h, wherein the sulfonating agent is aminosulfonic acid, the mass ratio of the sulfonating agent to the biomass-based carbon material is 0.5, and the concentration of the sulfonating agent is 2.5wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner, hydrothermally treated at 200℃ for 0.5h, filtered and washed, washed with deionized water until neutral, and dried at 120℃ for 8h to obtain a biomass carbon-based solid acid carrier;

[0124] (2) 0.1 g of support and 15 wt% of chloroauric acid and 50 wt% of ferric nitrate were added to water with a saturated water absorption capacity of 0.1 g of support. After stirring at 500 rpm for 6 h, the mixture was allowed to stand at room temperature for 48 h and dried at 150 °C for 8 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 200 °C for 10 h and then reduced at 500 °C for 5 h under a hydrogen atmosphere to obtain an Au-Fe bimetallic catalyst.

[0125] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0126] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of gold in the catalyst was 0.1% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 4.0 MPa of hydrogen gas was introduced. The temperature was raised to 260 °C, and the reaction was carried out at this temperature for 1 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 61%.

[0127] Example 4

[0128] (1) The biomass raw material is placed in a tube furnace and carbonized at 200°C for 10 hours under a nitrogen atmosphere, wherein: the biomass raw material is poplar wood powder; the obtained biomass-based carbon material is mixed with an aqueous solution of sulfonating agent at 1500 rpm for 0.2 hours, wherein the sulfonating agent is dodecylbenzene sulfonic acid, the mass ratio of the sulfonating agent to the biomass-based carbon material is 10, and the concentration of the sulfonating agent is 33 wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner, hydrothermally treated at 90°C for 12 hours, filtered and washed, washed with deionized water until neutral, and dried at 50°C for 72 hours to obtain a biomass carbon-based solid acid carrier;

[0129] (2) 0.1 g of support and 0.2 wt% of hexachloroplatinic acid and 5 wt% of molybdenum amino acid were added to water with a saturated water absorption capacity of 0.1 g of support. After stirring at 1200 rpm for 0.1 h, the mixture was allowed to stand at room temperature for 36 h and dried at 90 °C for 16 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 800 °C for 4 h and then reduced at 450 °C for 4 h under a hydrogen atmosphere to obtain a Pt-Mo bimetallic catalyst.

[0130] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0131] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of platinum in the catalyst was 25% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 1.0 MPa of hydrogen gas was introduced. The temperature was raised to 150 °C, and the reaction was carried out at this temperature for 24 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 59%.

[0132] Example 5

[0133] (1) The biomass raw material is placed in a tube furnace and carbonized at 500°C for 4 hours under a nitrogen atmosphere, wherein: the biomass raw material is cellulose; the obtained biomass-based carbon material is mixed with an aqueous sulfonating agent at 800 rpm for 1.5 hours, wherein the sulfonating agent is 98 wt% concentrated sulfuric acid, the mass ratio of the sulfonating agent to the biomass-based carbon material is 15, and the concentration of the sulfonating agent is 43 wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner, hydrothermally treated at 170°C for 6 hours, filtered and washed, washed with deionized water until neutral, and dried at 100°C for 12 hours to obtain a biomass-based solid acid carrier;

[0134] (2) 0.1 g of support and 5 wt% of rhodium chloride and 20 wt% of nickel nitrate were added to water with a saturated water absorption capacity of 0.1 g of support. After stirring at 1000 rpm for 1 h, the mixture was allowed to stand at room temperature for 16 h and dried at 110 °C for 14 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 500 °C for 6 h and then reduced at 350 °C for 6 h under a hydrogen atmosphere to obtain a Rh-Ni bimetallic catalyst.

[0135] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0136] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of rhodium in the catalyst was 8% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 2.5 MPa of hydrogen gas was introduced. The temperature was raised to 200 °C, and the reaction was carried out at this temperature for 8 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 62%.

[0137] Example 6

[0138] (1) The biomass raw material is placed in a tube furnace and carbonized at 400°C for 8 hours under a nitrogen atmosphere, wherein: the biomass raw material is birch powder; the obtained biomass-based carbon material is mixed with an aqueous sulfonating agent at 1200 rpm for 0.8 hours, wherein the sulfonating agent is p-toluenesulfonic acid, the mass ratio of the sulfonating agent to the biomass-based carbon material is 20, and the concentration of the sulfonating agent is 50 wt%. The mixed solution is transferred to a high-pressure hydrothermal autoclave with a polytetrafluoroethylene liner, hydrothermally treated at 190°C for 8 hours, filtered and washed, washed with deionized water until neutral, and dried at 80°C for 48 hours to obtain a biomass carbon-based solid acid carrier;

[0139] (2) 0.1 g of support and 3 wt% of ruthenium chloride and 40 wt% of nickel nitrate were added to water with a saturated water absorption capacity of 0.1 g of support. After stirring at 900 rpm for 1.5 h, the mixture was allowed to stand at room temperature for 30 h and dried at 130 °C for 9 h to obtain a bimetallic catalyst precursor. The precursor was calcined at 300 °C for 5 h and then reduced at 400 °C for 3 h under a hydrogen atmosphere to obtain a Ru-Ni bimetallic catalyst.

[0140] Application of bimetallic catalysts supported on biomass-based carbon-based solid acid supports in the decarboxylation of serine to prepare ethanolamine:

[0141] Serine, a bimetallic catalyst, and water were added to a 15 mL reactor, which was then closed. The amount of serine used was 1 mmol, the molar amount of ruthenium in the catalyst was 3% of the molar amount of serine, and the amount of water was 7 mL. The air inside the reactor was replaced five times with hydrogen gas, and then 1.5 MPa of hydrogen gas was introduced. The temperature was raised to 240 °C, and the reaction was carried out at this temperature for 4 h. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the catalyst was removed by centrifugation. Half of the reaction solution was rotary evaporated to remove the solvent water, and internal standard trioxane and deuterated water were added and mixed thoroughly. A sample was taken and subjected to NMR analysis. The other half of the reaction solution was diluted with acetonitrile, and internal standard mesitylene was added. A sample was taken and subjected to GC analysis. The conversion rate of serine and the GC yield of ethanolamine were calculated. The conversion rate of serine was 99%, and the yield of ethanolamine was 60%.

[0142] Example 7

[0143] The catalyst was prepared according to the conditions of Example 1. After reduction, the catalyst was used for the serine decarboxylation reaction. The difference from Example 1 is that after the reaction, the catalyst was separated by centrifugation and washed with water by centrifugation 5 times. The serine decarboxylation reaction was then circulated again. The catalyst was used in this way 5 times. The results are shown in Table 1.

[0144] Table 1

[0145]

[0146]

[0147] As shown in Table 1, the ruthenium-based catalyst maintained high catalytic activity for serine decarboxylation after five cycles, with the yield of ethanolamine remaining above 61%. The catalysts provided in Examples 2-6 also maintained high catalytic activity under the same conditions, with the yield of ethanolamine remaining above 60% after five cycles.

[0148] The catalyst used in this application exhibits synergistic effects between its bimetallic sites and the support, enabling the decarboxylation of serine to produce ethanolamine. The reaction is simple, the catalyst is easily separable, environmentally friendly, and demonstrates good cycle stability. This method and the catalyst used have broad application prospects.

[0149] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. The application of a bimetallic catalyst in the catalytic preparation of ethanolamine from serine, characterized in that, The bimetallic catalyst comprises a support and a bimetallic component supported on the support; The bimetallic component is selected from noble metals and non-noble metals; The precious metal is selected from at least one of Au, Pd, Pt, Rh, and Ru; The non-precious metal is selected from at least one of Mo, Fe, Co, Ni, and Cu; The noble metal in the catalyst has a mass content of 0.2~15 wt%. In the catalyst, the non-precious metal content is 5-50 wt%; The carrier is a biomass carbon-based solid acid; The biomass carbon-based solid acid is obtained through the following steps: 1) Carbonize biomass raw materials to obtain biomass-based carbon materials; 2) The biomass-based carbon material obtained in 1) is mixed with an aqueous solution containing a sulfonating agent, reacted in a sealed container, and dried to obtain the biomass-based solid acid; The biomass raw material is selected from at least one of starch, cellulose, chitin, corn cob powder, poplar powder, and birch powder.

2. The application according to claim 1, characterized in that, In the catalyst, the mass content of the noble metal is 1~8 wt%; The carbonization treatment temperature is 200~1000℃; The carbonization process takes 1 to 10 hours.

3. The application according to claim 1, characterized in that, In the catalyst, the non-precious metal content is 10~30 wt%; The carbonization treatment temperature is 300~800℃; The carbonization process takes 2 to 5 hours.

4. The application according to claim 1, characterized in that, The sulfonating agent is selected from at least one of 98 wt% concentrated sulfuric acid, p-toluenesulfonic acid, dodecylbenzenesulfonic acid, and aminosulfonic acid; The mass ratio of the sulfonating agent to the biomass-based carbon material obtained in step 1) is 0.5 to 30; In the aqueous solution containing the sulfonating agent, the concentration of the sulfonating agent is 2.5~60 wt%; The reaction is a hydrothermal reaction; The reaction temperature is 90~200℃; The reaction time is 0.5~15h; The drying temperature is 50~120℃; The drying time is 8 to 72 hours.

5. The application according to claim 1, characterized in that, The reaction temperature is 150~180℃; The reaction time is 4-12 hours; The drying temperature is 90~110℃; The drying time is 10-24 hours.

6. The application according to any one of claims 1 to 5, characterized in that, Its preparation method includes the following steps: The support was immersed in an aqueous solution containing a bimetallic precursor, then dried, calcined, and reduced to obtain the bimetallic catalyst.

7. The application according to claim 6, characterized in that, The bimetallic component precursor is selected from noble metal precursors and non-noble metal precursors; The noble metal precursor is selected from at least one of chloroauric acid, palladium chloride, hexachloroplatinic acid, rhodium chloride, and ruthenium chloride; The non-precious metal precursor is selected from at least one of ammonium molybdate, ferric nitrate, cobalt acetate, nickel nitrate, and copper chloride; The impregnation is an equal-volume impregnation; The carrier is a biomass carbon-based solid acid; The biomass carbon-based solid acid is obtained through the following steps: 1) Carbonize biomass raw materials to obtain biomass-based carbon materials; 2) The biomass-based carbon material obtained in 1) is mixed with an aqueous solution containing a sulfonating agent, reacted in a sealed container, and dried to obtain the biomass-based solid acid; The biomass raw material is selected from at least one of starch, cellulose, chitin, corn cob powder, poplar powder, and birch powder.

8. The application according to claim 6, characterized in that, The drying temperature is 90~150℃; The drying time is 8-16 hours; The calcination temperature is 200~800℃; The calcination time is 2-10 hours; The reducing atmosphere is a hydrogen atmosphere; The reduction temperature is 200~500℃; The restoration time is 2 to 8 hours.

9. The application according to claim 6, characterized in that, The drying temperature is 100~120℃; The drying time is 10-12 hours; The calcination temperature is 400~600℃; The calcination time is 2-8 hours; The reduction temperature is 300~450℃; The restoration time is 2-5 hours.

10. A method for catalytically preparing ethanolamine from serine, characterized in that, Includes the following steps: Hydrogen gas is introduced into a mixture containing serine, a catalyst, and water to carry out a decarboxylation reaction, yielding ethanolamine. The catalyst is selected from the catalysts used in the applications described in any one of claims 1 to 9.

11. The method according to claim 10, characterized in that, The molar amount of the catalyst is 0.1 to 25% of the molar amount of the serine.

12. The method according to claim 10, characterized in that, The pressure of the hydrogen gas is 1~4 MPa; The temperature for the decarboxylation reaction is 150~260℃; The decarboxylation reaction takes 1 to 24 hours.

13. The method according to claim 10, characterized in that, The pressure of the hydrogen gas is 2~3 MPa; The temperature for the decarboxylation reaction is 180~220℃; The decarboxylation reaction takes 1 to 12 hours.

Citation Information

Patent Citations

  • Preparation method of Ni-based catalyst modified by aid Pt supported by multi-wall carbon nanotube as carrier and application