A method for preparing a hierarchical pore catalyst and application thereof

By preparing a hierarchical porous molecular sieve catalyst, the problems of low ethylbenzene conversion and severe side reactions in the existing technology were solved, and the effects of high selectivity for xylene and reduced cracking products were achieved, with higher isomerization activity.

CN118122366BActive Publication Date: 2026-11-10DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211433843.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2026-11-10
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

Existing catalysts exhibit low ethylbenzene conversion and severe side reactions during xylene isomerization, making it difficult to achieve high selectivity for para-xylene and reduce pyrolysis and polymer products.

Method used

A method for preparing a hierarchical porous molecular sieve catalyst is adopted, which involves treating microporous molecular sieves with a chelation-alkaline medium, combining ammonium exchange and binder molding, loading platinum and then calcining and reducing to form a hierarchical porous structure, and regulating acidity to control the cracking reaction.

Benefits of technology

It improves the selectivity of xylene and the conversion rate of ethylbenzene, reduces cracking and polymer products, and has higher isomerization activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003946182690000071
    Figure BDA0003946182690000071
  • Figure BDA0003946182690000072
    Figure BDA0003946182690000072
  • Figure BDA0003946182690000073
    Figure BDA0003946182690000073
Patent Text Reader

Abstract

The application discloses a preparation method of a multi-level hole molecular sieve catalyst and application thereof. The preparation method comprises the following steps: a) adding microporous molecular sieve into a chelate-alkaline medium, stirring I, centrifugal washing, drying I, calcining I, and obtaining substance I; b) adding the substance I into an ammonium salt solution, ammonium exchange, centrifugal washing, drying II, calcining II, and obtaining a porous molecular sieve; c) mixing the porous molecular sieve with a binder, extruding into a strip, calcining III, and crushing to obtain a carrier; and d) adding the carrier into a platinum salt solution, equal-volume impregnation, drying III, calcining IV, and reduction to obtain the multi-level hole molecular sieve catalyst. The catalyst prepared by the method is used for C8 aromatic hydrocarbon isomerization reaction, has higher xylene selectivity, increased ethylbenzene conversion rate, obviously reduced cracking and polymer product, and has higher isomerization activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a method for preparing a hierarchical porous catalyst and its application, belonging to the field of catalyst synthesis. Background Technology

[0002] p-Xylene (also known as "para-xylene" or "PX") is an important chemical raw material, mainly used in the production of terephthalic acid and dimethyl terephthalate, and also has applications in coatings, dyes, pesticides, and pharmaceuticals. With the development of these industries, the demand for PX has grown rapidly. Currently, the main process technology for increasing PX production is xylene isomerization, which converts lower-value m-xylene and o-xylene into p-xylene.

[0003] CN111744542A discloses a core-shell type xylene isomerization catalyst. The core / shell type catalyst is ZSM-5 molecular sieve / alumina, with 0.01-0.2 wt% of noble metal platinum supported, which improves the activity and selectivity of C8 aromatic isomerization. However, the conversion rate of ethylbenzene is low, not reaching 70%.

[0004] CN106925339A discloses a method for preparing a hierarchical porous molecular sieve catalyst for the isomerization reaction of xylene in C8 aromatics. The catalyst uses a nano-molecular sieve loaded with two groups of metals and solves the problems of high xylene loss rate and serious side reactions such as hydrogenation cracking and disproportionation.

[0005] CN105582978A discloses a catalyst prepared using acid-modified ZSM-5 molecular sieve, which is used in xylene isomerization reaction and achieves higher isomerization activity.

[0006] Therefore, a catalyst with high selectivity for p-xylene, high conversion rate of ethylbenzene, and reduced cracking and polymer products is needed. Summary of the Invention

[0007] The purpose of this invention is to provide a catalyst for the isomerization reaction of aromatic hydrocarbons and its preparation method. The prepared catalyst is used for the isomerization reaction of C8 aromatic hydrocarbons, exhibiting high selectivity for xylene, increased ethylbenzene conversion, and a significant reduction in cracking and polymer products, thus possessing higher isomerization activity.

[0008] According to one aspect of this application, a method for preparing a hierarchical porous molecular sieve catalyst is provided, comprising the following steps:

[0009] a) Add the microporous molecular sieve to the chelating-alkaline medium, stir I, centrifuge and wash, dry I, calcine I, to obtain substance I;

[0010] b) Add substance I to an ammonium salt solution, perform ammonium exchange, centrifuge and wash, dry II, calcine II, and obtain a porous molecular sieve;

[0011] c) The porous molecular sieve is mixed with a binder, extruded into strips, calcined (III), and pulverized to obtain a carrier;

[0012] d) The support is added to a platinum salt solution, impregnated with an equal volume, dried (III), calcined (IV), and reduced to obtain the hierarchical porous molecular sieve catalyst.

[0013] Optionally, the mesopore size of the hierarchical porous molecular sieve catalyst is 5–20 nm.

[0014] Optionally, the mesopore size of the hierarchical molecular sieve catalyst is any value or a range between two of 5 nm, 10 nm, 13 nm, 15 nm, and 20 nm.

[0015] Optionally, the microporous molecular sieve is selected from any one of ZSM-5 molecular sieve, ZSM-11 molecular sieve, and β molecular sieve.

[0016] Optionally, the silicon-to-aluminum ratio of the ZSM-5 molecular sieve is 20 to 50;

[0017] The silicon-aluminum ratio of the ZSM-11 molecular sieve is 40–70.

[0018] The silica-to-alumina ratio of the β-zeolite is 5–20.

[0019] Optionally, the chelating-alkaline medium includes a chelating agent and an alkaline solution.

[0020] The chelating agent is selected from at least one of ethylenediaminetetraacetic acid tetrasodium, ethylenediaminetetraacetic acid disodium, sodium citrate, and sodium gluconate;

[0021] The alkaline solution is selected from at least one of NaOH, LiOH, KOH, CsOH, and Na2CO3.

[0022] Optionally, the chelating-alkaline medium is prepared by mixing a chelating agent with an alkaline solution to obtain the chelating-alkaline medium.

[0023] Optionally, in the chelating-alkaline medium, the concentration of the chelating agent is 0.01–0.5 mol / L;

[0024] The concentration of the alkaline solution is 0.05–1 mol / L.

[0025] Optionally, the lower limit of the concentration of the chelating agent is independently selected from 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, and 0.2 mol / L, and the upper limit is independently selected from 0.5 mol / L, 0.45 mol / L, 0.4 mol / L, 0.35 mol / L, and 0.3 mol / L.

[0026] Optionally, the lower limit of the concentration of the alkaline solution is independently selected from 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, and the upper limit is independently selected from 1 mol / L, 0.9 mol / L, 0.8 mol / L, 0.7 mol / L, 0.6 mol / L, 0.5 mol / L.

[0027] Optionally, in the chelating-alkaline medium, the molar ratio of the chelating agent to the alkaline solution is 1:0.1 to 100.

[0028] Optionally, in step a), the solid-liquid ratio of the microporous molecular sieve to the chelating-alkaline medium is 1:20 to 40 g / mL.

[0029] Optionally, in step a), the lower limit of the solid-liquid ratio of the microporous molecular sieve to the chelating-alkaline medium is independently selected from 1:20 g / mL, 1:22 g / mL, 1:24 g / mL, 1:26 g / mL, 1:28 g / mL, and 1:29 g / mL, and the upper limit is independently selected from 1:40 g / mL, 1:38 g / mL, 1:36 g / mL, 1:34 g / mL, 1:32 g / mL, and 1:30 g / mL.

[0030] Optionally, in step a), the temperature of stirring I is 30–90°C, and the stirring time is 10–60 min.

[0031] Optionally, in step a), the temperature of stirring I is selected from any value or a range between two values ​​from 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, and 90℃.

[0032] Optionally, in step a), the stirring time I is selected from any value or a range between two values ​​of 10 min, 20 min, 30 min, 40 min, 50 min, and 60 min.

[0033] Optionally, in step a), the temperature of drying I is 80–120°C.

[0034] Optionally, in step a), the temperature of the drying I is selected from any value or a range between two values ​​of 80°C, 90°C, 100°C, 110°C, and 120°C.

[0035] Optionally, the temperature of the calcination I is 400–600°C, and the calcination time is 2–5 hours.

[0036] Optionally, the temperature of the roasting I is selected from any value or a range between two values ​​of 400℃, 450℃, 500℃, 550℃, and 600℃.

[0037] Optionally, the roasting time I is selected from any value of 2h, 3h, 4h, 5h or a range between two values.

[0038] Optionally, in step b), the ammonium salt solution is selected from at least one of ammonium nitrate, ammonium chloride, and ammonium carbonate.

[0039] Optionally, the concentration of the ammonium salt solution is 0.5 to 1 mol / L.

[0040] Optionally, the lower limit of the concentration of the ammonium salt solution is independently selected from 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, and 0.7 mol / L, and the upper limit is independently selected from 1 mol / L, 0.95 mol / L, 0.9 mol / L, 0.85 mol / L, 0.8 mol / L, and 0.7 mol / L.

[0041] Optionally, the ammonium exchange temperature is 70–95°C, the ammonium exchange time is 1–3 hours, and the ammonium exchange is performed 1–5 times.

[0042] Optionally, the ammonium exchange temperature is selected from any value or a range between two of 70°C, 75°C, 80°C, 85°C, 90°C, and 95°C.

[0043] Optionally, the ammonium exchange time is selected from any value of 1h, 1.5h, 2h, 2.5h, 3h or a range between two values.

[0044] Optionally, the number of ammonium exchanges is selected from any value among 1, 2, 3, 4, and 5.

[0045] Optionally, the temperature of the drying II process is 80–120°C.

[0046] Optionally, the temperature of the drying II is selected from any value of 80°C, 90°C, 100°C, 110°C, or 120°C, or a range between two values.

[0047] Optionally, the temperature of the second calcination is 400–600°C, and the calcination time is 2–5 hours.

[0048] Optionally, the temperature of the roasting II is selected from any value of 400℃, 450℃, 500℃, 550℃, 600℃ or a range between two values.

[0049] Optionally, the roasting time II is selected from any value of 2h, 2.5h, 3h, 3.5h, 4h, 5h or a range between two values.

[0050] Optionally, in step c), the adhesive is selected from at least one of alumina, silica gel, and clay.

[0051] Optionally, the mass ratio of the porous molecular sieve to the binder is 1:0.1 to 10.

[0052] Optionally, the lower limit of the mass ratio of the porous molecular sieve to the binder is independently selected from 1:0.1, 1:0.5, 1:1, 1:2, 1:3, and the upper limit is independently selected from 1:10, 1:9, 1:8, 1:7, 1:6, 1:5.

[0053] Optionally, an acidic aqueous solution is added during the extrusion molding process of the porous molecular sieve and the binder, wherein the acid in the acidic aqueous solution includes at least one of nitric acid, hydrochloric acid, and acetic acid.

[0054] Optionally, the temperature of the third calcination is 400–600°C, and the calcination time is 2–5 hours.

[0055] Optionally, the temperature of the roasting III is selected from any value or a range between two of 400°C, 450°C, 500°C, 550°C, and 600°C.

[0056] Optionally, the roasting time III is selected from any value of 2h, 2.5h, 3h, 3.5h, 4h, 5h or a range between two values.

[0057] Optionally, in step d), the platinum salt solution is selected from at least one of chloroplatinic acid and chloroplatinic acid amine.

[0058] Optionally, the concentration of the platinum salt solution is 5 × 10⁻⁶. -4 ~0.2mol / L.

[0059] Optionally, the lower concentration limit of the platinum salt solution is independently selected from 5 × 10⁻⁶. -4 mol / L, 5×10 -3 mol / L, 1×10 -2 mol / L, 3×10 -2 mol / L, 5×10 -2 mol / L, with the upper limit independently selected from 5×10 -2 mol / L, 7×10 -2 mol / L, 9×10 - 2 mol / L, 0.1mol / L, 0.2mol / L.

[0060] Optionally, the temperature of the equal-volume impregnation is 25–50°C, and the time of the equal-volume impregnation is 5–20 h.

[0061] Optionally, the temperature for the equal-volume impregnation is selected from any value of 25°C, 30°C, 35°C, 40°C, or 50°C, or a range between two values.

[0062] Optionally, the time for the equal-volume impregnation is selected from any value of 5h, 8h, 12h, 15h, 20h or a range between two values.

[0063] Optionally, the temperature of the drying III process is 50–120°C, and the drying time is 3–30 hours.

[0064] Optionally, the temperature of the drying III is selected from any value of 50°C, 70°C, 90°C, 100°C, or 120°C, or a range between two values.

[0065] Optionally, the drying time III is selected from any value of 3h, 5, 12h, 24h, 30h or a range between two values.

[0066] Optionally, the temperature of the calcination IV is 400–600°C, and the calcination time of the IV is 2–5 hours.

[0067] Optionally, the temperature of the calcination IV is selected from any value of 400°C, 450°C, 500°C, 550°C, and 600°C, or a range between two values.

[0068] Optionally, the calcination time IV is selected from any value of 2h, 2.5h, 3h, 3.5h, 4h, 5h or a range between two values.

[0069] Optionally, the reduction temperature is 450–500°C, the reduction time is 1–5 hours, and the reduction atmosphere is hydrogen.

[0070] Optionally, the reduction temperature is selected from any value or a range between two values ​​from 450℃, 460℃, 470℃, 480℃, 490℃, and 500℃.

[0071] Optionally, the restoration time is selected from any value of 1h, 2h, 3h, 4h, 5h or a range between two values.

[0072] According to another aspect of this application, a method for isomerization of aromatic hydrocarbons is provided, wherein a feedstock containing ethylbenzene, p-xylene, o-xylene and m-xylene is reacted with a catalyst to obtain xylene isomerization products.

[0073] The catalyst is selected from the catalysts obtained by the above preparation method.

[0074] Optionally, the reaction temperature is 300–450°C.

[0075] Optionally, the temperature of the reaction is selected from any value of 300°C, 350°C, 400°C, 450°C, or a range between two values.

[0076] Optionally, the space velocity of the raw material is 5 to 30 h⁻¹. -1 .

[0077] Optionally, the space velocity of the raw material is selected from 5 h. -1 10h -1 15h -1 20h -1 30h -1 Any value in the range or between two values.

[0078] Optionally, the mass ratio of ethylbenzene, o-xylene, and m-xylene in the raw materials is 1:5-7:2-4.

[0079] Optionally, the reaction is carried out in a fixed-bed reactor, wherein the fixed-bed reactor comprises at least one.

[0080] The beneficial effects that this application can produce include:

[0081] 1) The preparation method provided in this application uses a chelation-alkaline medium treatment method to obtain a hierarchical porous molecular sieve with excellent reaction diffusion performance. The acidity of the molecular sieve can be adjusted by controlling the degree of ammonium exchange, thereby effectively controlling the occurrence of cracking reaction.

[0082] 2) The method for isomerization of aromatics provided in this application prepares a catalyst for the isomerization reaction of C8 aromatics. The catalyst has high selectivity for xylene, increased conversion of ethylbenzene, and significantly reduced cracking and polymer products, and has higher isomerization activity. Attached Figure Description

[0083] Figure 1 The images shown are scanning electron microscope (SEM) images of the sample prepared in Example 1 of this application, wherein the left image is a 200,000x magnified SEM image and the right image is a 20,000x magnified SEM image.

[0084] Figure 2 The nitrogen adsorption diagrams for the sample prepared in Example 1 of this application are shown in figure a), where figure a) is the nitrogen adsorption isotherm and figure b) is the BJH pore size distribution curve. Detailed Implementation

[0085] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0086] Unless otherwise specified, the raw materials and solvents used in the embodiments of this application were all purchased commercially.

[0087] The analysis method in the embodiments of this application is as follows:

[0088] This invention utilizes a Mack ASAP 2020PLUS HD88 physical adsorption analyzer to characterize the nitrogen physical adsorption of hierarchical porous molecular sieves. The analytical conditions are as follows: 0.10 g of molecular sieve is loaded into a quartz adsorption tube and vacuum-treated at 350 °C for 10 h to remove adsorbed moisture and impurities from the molecular sieve material. Nitrogen adsorption / desorption experiments are conducted at 77.4 K. The total specific surface area of ​​the sample is calculated using the Brunauer-Emmett-Teller (BET) equation, and the micropore specific surface area and micropore volume of the molecular sieve sample are calculated using the t-plot method. At P / P0 = 0.99, the total pore volume of the sample is obtained from the volume of adsorbed nitrogen. The mesopore specific surface area is calculated by the difference between the total specific surface area and the micropore specific surface area, and the mesopore volume is calculated by the difference between the total pore volume and the micropore volume. The mesopore distribution information of the sample is obtained using the BJH model.

[0089] The isomerization activity, xylene yield, and ethylbenzene conversion rates in the embodiments of this application are calculated as follows:

[0090]

[0091]

[0092]

[0093] Example 1: Preparation of Hierarchical Porous Molecular Sieves

[0094] Take 600 ml of an aqueous solution containing 0.2 mol / L NaOH and 0.3 mol / L Na4EDTA (tetrasodium ethylenediaminetetraacetate), heat it in a water bath to 65°C, add 20.00 g of microporous ZSM-5 molecular sieve (Si / Al = 35), stir at 65°C for 30 min, then centrifuge and wash until the washing liquid is neutral. Dry the obtained molecular sieve solid at 100°C for 12 h, and calcine at 550°C for 3 h to obtain substance I. Take 280 ml of 0.8 mol / L ammonium nitrate solution, preheat it to 85°C, add 14.0 g of substance I, stir and exchange for 2 h, repeat the exchange 3 times, then centrifuge and wash, dry at 100°C for 12 h, and finally calcine at 550°C for 3 h. The obtained solid is the multi-level porous molecular sieve, denoted as HZ1.

[0095] Figure 1 This is a scanning electron microscope image of HZ1 prepared in this embodiment, based on... Figure 1 The left figure shows that the prepared hierarchical porous molecular sieve has a dense mesoporous structure, while the right figure shows that the hierarchical porous molecular sieve obtained by this method can maintain a certain crystal structure.

[0096] Figure 2The nitrogen adsorption diagram of HZ1 prepared in this embodiment shows that its adsorption-desorption isotherm has obvious hysteresis loop, indicating that it has a mesoporous structure.

[0097] As shown in Figure b), the pore size of its mesoporous structure is between 4 and 18 nm, with a peak value of around 11 nm.

[0098] Example 2: Preparation of Hierarchical Porous Molecular Sieves

[0099] The hierarchical porous molecular sieve was prepared according to the method of Example 1, except that the alkali was KOH, the chelating agent was sodium citrate, and the ammonium exchange was performed once. The resulting solid was the hierarchical porous molecular sieve, denoted as HZ2.

[0100] Example 3: Preparation of Hierarchical Porous Molecular Sieves

[0101] Multi-level porous molecular sieves were prepared according to the method in Example 1, except that the original molecular sieve used was a β molecular sieve (Si / Al = 12), the concentration of the alkaline solution was 0.1 mol / L, the alkaline treatment temperature was 50°C, the chelating agent was sodium citrate, and the resulting solid was the multi-level porous molecular sieve, denoted as HZ3.

[0102] Example 4: Preparation of Hierarchical Porous Molecular Sieves

[0103] The hierarchical porous molecular sieve was prepared according to the method in Example 1, except that the original molecular sieve used was ZSM-11 molecular sieve (Si / Al = 55), the alkali was LiOH, the concentration of the alkali solution was 0.5 mol / L, the concentration of the ammonium salt solution was 0.5 mol / L, the number of exchanges was 2, and the resulting solid was the hierarchical porous molecular sieve, denoted as HZ4.

[0104] Example 5: Preparation of Catalyst

[0105] 7.00g of hierarchical porous molecular sieve HZ1 and 3.00g of alumina powder were physically mixed. After uniform mixing, an appropriate amount of 10wt% nitric acid solution was added and mixed evenly. The mixture was then placed in a mold for extrusion molding. After drying the strips, they were calcined at 500℃ for 2h and then crushed to 20-40 mesh. The resulting solid was the support for the catalyst and was denoted as S1. 17ml of chloroplatinic acid aqueous solution containing 0.002g of platinum was prepared. The resulting liquid was the precursor solution. 10.00g of support was weighed and the precursor solution was added to the support. The mixture was impregnated at room temperature for 12h, dried at 60℃ for 24h, calcined at 550℃ for 4h, and then reduced with hydrogen at 480℃ for 4h. The resulting sample was denoted as Cat1, in which the Pt loading calculated based on the support was 0.02wt%.

[0106] Example 6 Preparation of Catalyst

[0107] The catalyst was prepared according to the method of Example 5, except that the platinum content in the prepared chloroplatinic acid aqueous solution was 0.01 g, and the resulting sample was denoted as Cat2, in which the Pt loading calculated based on the support was 0.1 wt%.

[0108] Example 7 Preparation of Catalyst

[0109] The catalyst was prepared according to the method of Example 5, except that the mass ratio of hierarchical porous molecular sieve to alumina was 3:2. The resulting catalyst support was denoted as S2, and the resulting sample was denoted as Cat3. The Pt loading calculated based on the support was 0.02 wt%.

[0110] Example 8 Preparation of Catalyst

[0111] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ2, the resulting catalyst support was designated as S3, and the resulting sample was designated as Cat4, wherein the Pt loading calculated based on the support was 0.02 wt%.

[0112] Example 9 Preparation of Catalyst

[0113] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ2, the mass ratio of the hierarchical porous molecular sieve to alumina was 1:1, the resulting catalyst support was denoted as S4, and the resulting sample was denoted as Cat5, wherein the Pt loading calculated based on the support was 0.02wt%.

[0114] Example 10 Preparation of Catalyst

[0115] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ3, the resulting catalyst support was designated as S5, the platinum content in the prepared chloroplatinic acid aqueous solution was 0.005 g, and the resulting sample was designated as Cat6, wherein the Pt loading calculated based on the support was 0.05 wt%.

[0116] Example 11 Preparation of Catalyst

[0117] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ3, the mass ratio of hierarchical porous molecular sieve to alumina was 3:2, the resulting catalyst support was designated as S6, and the resulting sample was designated as Cat7, wherein the Pt loading calculated based on the support was 0.02 wt%.

[0118] Example 12 Preparation of Catalyst

[0119] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ4, the resulting catalyst support was designated as S7, and the resulting sample was designated as Cat8, wherein the Pt loading calculated based on the support was 0.02 wt%.

[0120] Example 13 Preparation of Catalyst

[0121] The catalyst was prepared according to the method of Example 5, except that the hierarchical porous molecular sieve used was HZ4, the mass ratio of the hierarchical porous molecular sieve to alumina was 3:2, the resulting catalyst support was denoted as S8, and the resulting sample was denoted as Cat9, wherein the Pt loading calculated based on the support was 0.02wt%.

[0122] Example 14 Preparation of Catalyst

[0123] The catalyst was prepared according to the method of Example 5, except that the calcination temperature after impregnation with platinum was 450°C, and the resulting sample was designated Cat10, wherein the Pt loading calculated based on the support was 0.02 wt%.

[0124] Preparation of catalyst in Comparative Example 1

[0125] The catalyst was prepared according to the method in Example 5, except that the molecular sieve used was a primitive microporous molecular sieve that was extruded and the resulting sample was denoted as Comp1.

[0126] Preparation of catalyst in Comparative Example 2

[0127] Prepare 17 ml of chloroplatinic acid aqueous solution containing 0.002 g of platinum. The resulting liquid is the precursor solution. Weigh 10.00 g of hierarchical porous molecular sieve HZ1. Add the precursor solution to the support, soak at room temperature for 12 h, dry at 60 °C for 24 h, calcine at 550 °C for 4 h, and then reduce with hydrogen at 480 °C for 4 h. The resulting sample is denoted as Comp2, in which the Pt loading calculated based on the support is 0.02 wt%.

[0128] The components of each catalyst are shown in Table 1.

[0129] Table 1

[0130]

[0131]

[0132] Examples 15-26: Application of the catalyst

[0133] The catalyst obtained in this invention was evaluated for its catalytic performance using a fixed-bed reactor. 0.3 g of catalyst was loaded, and the evaluation was conducted using C8 aromatic hydrocarbons as feedstock. The isomers in the C8 aromatic hydrocarbons had the following mass fractions: ethylbenzene 10%, m-xylene 60%, and o-xylene 30%. The evaluation conditions were 360 ​​°C, 0.5 MPa, and a feedstock mass flow rate of 10 h⁻¹. -1 The hydrogen / hydrocarbon molar ratio was 1.10. The catalysts used in each example and the reaction results are shown in Table 2.

[0134] Table 2

[0135] Example catalyst PX / ∑X(%) Xy(%) EBC (%) 15 Cat1 23.81 98.3 70.5 16 Cat2 23.94 99.4 75.2 17 Cat3 23.73 97.7 66.4 18 Cat4 23.91 99.1 71.9 19 Cat5 20.52 97.5 65.7 20 Cat6 22.84 98.3 73.8 21 Cat7 20.62 95.9 62.5 22 Cat8 22.94 97.8 67.7 23 Cat9 21.67 96.4 65.3 24 Cat10 23.53 98.6 68.4 25 Comp1 17.25 86.5 47.8 26 Comp2 20.42 82.6 45.6

[0136] As shown in Table 2, the catalyst prepared by the present invention with hierarchical porous molecular sieve as the active component has higher xylene isomerization activity (PX / ∑X) and higher xylene yield (Xy) compared with the catalyst prepared in the comparative example. This indicates that the catalyst effectively reduces the generation of side reactions, has high selectivity for xylene, and also has a high ethylbenzene conversion rate (EBC), which is beneficial to the separation of subsequent products in the production process.

[0137] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a hierarchical porous molecular sieve catalyst, characterized in that, Includes the following steps: a) Add the microporous molecular sieve to a chelating-alkaline medium including a chelating agent and an alkaline solution, stir I, centrifuge and wash, dry I, calcine I, to obtain substance I; wherein, the chelating agent is selected from at least one of ethylenediaminetetraacetic acid tetrasodium, ethylenediaminetetraacetic acid disodium, sodium citrate, and sodium gluconate. b) Add substance I to an ammonium salt solution, perform ammonium exchange, centrifuge and wash, dry II, calcine II, and obtain a porous molecular sieve; c) The porous molecular sieve is mixed with a binder, extruded into strips, calcined (III), and pulverized to obtain a carrier; d) The support is added to a platinum salt solution, impregnated with an equal volume, dried (III), calcined (IV), and reduced to obtain the hierarchical porous molecular sieve catalyst.

2. The preparation method according to claim 1, characterized in that, The mesopore size of the hierarchical porous molecular sieve catalyst is 5~20 nm.

3. The preparation method according to claim 1, characterized in that, The microporous molecular sieve is selected from any one of ZSM-5 molecular sieve, ZSM-11 molecular sieve, and β molecular sieve. The silicon-aluminum ratio of the ZSM-5 molecular sieve is 20~50; The silicon-aluminum ratio of the ZSM-11 molecular sieve is 40~70; The silica-to-alumina ratio of the β-molecular sieve is 5-20; The alkali in the alkaline solution is selected from at least one of NaOH, LiOH, KOH, CsOH, and Na2CO3; The preparation method of the chelating-alkaline medium is as follows: mixing the chelating agent with an alkaline solution and heating to obtain the chelating-alkaline medium; In the chelating-alkaline medium, the concentration of the chelating agent is 0.01~0.5 mol / L; The concentration of the alkaline solution is 0.05~1 mol / L; In the chelating-alkaline medium, the molar ratio of the chelating agent to the alkali in the alkaline solution is 1:0.1~100.

4. The preparation method according to claim 1, characterized in that, In step a), the solid-liquid ratio of the microporous molecular sieve to the chelating-alkaline medium is 1:20~40g / mL; In step a), the temperature of stirring I is 30~90℃, and the stirring time is 10~60min; In step a), the temperature of drying I is 80~120℃; In step a), the temperature of calcination I is 400~600℃, and the calcination time is 2~5h.

5. The preparation method according to claim 1, characterized in that, In step b), the ammonium salt solution is selected from at least one of ammonium nitrate, ammonium chloride, and ammonium carbonate; The concentration of the ammonium salt solution is 0.5~1 mol / L; The ammonium exchange temperature is 70~95℃, the ammonium exchange time is 1~3h, and the ammonium exchange is performed 1~5 times. The temperature of the drying II process is 80~120℃; The temperature of the second calcination is 400~600℃, and the time of the second calcination is 2~5h.

6. The preparation method according to claim 1, characterized in that, In step c), the adhesive is selected from at least one of alumina, silica gel, and clay; The mass ratio of the porous molecular sieve to the binder is 1:0.1~10; An acidic aqueous solution is added during the extrusion molding process of the porous molecular sieve and the binder. The acid in the acidic aqueous solution includes at least one of nitric acid, hydrochloric acid, and acetic acid. The temperature of the third calcination is 400~600℃, and the calcination time is 2~5h.

7. The preparation method according to claim 1, characterized in that, In step d), the platinum salt solution is selected from at least one of chloroplatinic acid and chloroplatinic acid amine; The concentration of the platinum salt solution is 5 × 10⁻⁶. -4 ~0.2 mol / L; The temperature for the equal-volume impregnation is 25~50℃, and the time for the equal-volume impregnation is 5~20h; The temperature of the drying process III is 50~120℃, and the drying time of the drying process III is 3~30h; The calcination IV temperature is 400~600℃, and the calcination IV time is 2~5h; The reduction temperature is 450~500℃, the reduction time is 1~5 h, and the reduction atmosphere is hydrogen.

8. A method for isomerization of aromatic hydrocarbons, characterized in that, The raw materials containing ethylbenzene, p-xylene, o-xylene and m-xylene are reacted with a catalyst to obtain xylene isomerization products; The catalyst is selected from the catalysts obtained by the preparation method according to any one of claims 1 to 7.

9. The method according to claim 8, characterized in that, The reaction temperature is 300~450℃; The space velocity of the raw material is 5-30 h⁻¹. -1 ; The mass ratio of ethylbenzene, o-xylene, and m-xylene in the raw materials is 1: 5~7: 2~4.

10. The method according to claim 8, characterized in that, The reaction is carried out in a fixed-bed reactor, which contains at least one fixed-bed reactor.

Citation Information

Patent Citations

  • Preparation method of multistage molecular sieve catalyst for isomerization reaction of xylene in C8 aromatics

    CN106925339A

  • Xylene isomerization catalyst and preparation method

    CN111744542A

  • Preparation method of xylene isomerization catalyst

    CN105582978A

  • Method for preparing multi-stage pore Y molecular sieve through H4EDTA-NaOH co-treatment

    CN110065952A

  • Preparation method of hierarchical pore molecular sieve

    CN114620742A