Method for preventing the erosion of the bottom of a converter with high flow of bottom blown co2

By designing novel bottom-blowing components and gas flow control, the problem of furnace bottom erosion during high-flow-rate bottom-blowing CO2 in converters was solved, extending the converter's service life, improving decarbonization efficiency and CO2 recovery rate, and reducing smelting costs.

CN118127261BActive Publication Date: 2026-11-10SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410139528.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-01
Publication Date
2026-11-10
Estimated Expiration
2044-02-01

AI Technical Summary

Technical Problem

When the converter is blown with a large flow rate of bottom CO2, the bottom of the furnace is severely eroded, which affects the furnace life and production cost. Existing technologies, such as sacrificing furnace life or quickly replacing bottom blowing gas supply components, cannot effectively solve this problem.

Method used

A novel bottom-blowing assembly is designed, in which CO2 is injected through the central tube and inert gases such as N2 or Ar are injected through the ring tube. The gas flow ratio and gas supply intensity are controlled at different smelting stages. The inert gases are used to isolate CO2 from contact with the furnace bottom refractory material, forming a clustering effect to promote the decarburization reaction.

Benefits of technology

It effectively prevents furnace bottom erosion, extends converter life, increases decarburization speed, shortens smelting time, realizes CO2 recovery and utilization, reduces costs and carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127261B_ABST
    Figure CN118127261B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preventing erosion of the converter bottom by high-flow-rate bottom-blown CO2, comprising: uniformly distributing multiple bottom-blowing components along the circumference of a concentric circle of the converter bottom with a diameter of 0.4 to 0.6D; each bottom-blowing component is designed to include a central pipe and a ring pipe; in the early stage of smelting, CO2 is injected through the central pipe and N2 is injected through the ring pipe, with a gas supply intensity of 0.10 to 0.18 Nm. 3 / (min·t), the gas flow ratio of CO2 to N2 is 4:1; during the middle stage of smelting, CO2 is injected through the central pipe and N2 is injected through the ring pipe, with a gas supply intensity of 0.08~0.16Nm. 3 / (min·t), the gas flow ratio of CO2 to N2 is 3:1; in the later stage of smelting, CO2 is injected through the central pipe and Ar gas is injected through the ring pipe, with a gas supply intensity of 0.15~0.20Nm. 3 / (min·t), the gas flow ratio of CO2 to Ar is 5:1. This invention utilizes inert gas injected through a ring pipe to isolate the contact between CO2 injected through a central pipe and the refractory material at the furnace bottom, effectively reducing the erosion rate of the furnace bottom. While achieving high-flow-rate bottom blowing of CO2 throughout the process, it avoids furnace bottom erosion, and simultaneously promotes the stirring effect of the molten pool and realizes the recovery and utilization of CO2, thereby reducing smelting costs and carbon emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of converter steelmaking technology, and more specifically relates to a method for preventing the bottom erosion of a converter with high-flow-rate bottom-blown CO2. Background Technology

[0002] Increasing the bottom blowing intensity in converters can enhance molten pool stirring, improve molten pool kinetics, promote slag-steel interface reactions, and provide favorable kinetic conditions for dephosphorization and oxygen control. Steel plants both domestically and internationally have conducted research on high-flow-rate bottom blowing in converters, with bottom blowing gas supply intensity ≥ 0.10 Nm³. 3 The concentration of steel feed per ton (min·t) can improve the stirring intensity of the converter and reduce the oxidizability of molten steel. The consumption of steel feed is reduced by 3-5 kg / t, and the oxygen content at the end of the converter melt is reduced by more than 100 ppm, achieving remarkable results.

[0003] Large-scale CO2 emissions are a major cause of the greenhouse effect; approximately 2 tons of CO2 are emitted for every ton of steel produced. Efficient CO2 recovery and utilization are crucial for reducing greenhouse gas emissions. Therefore, many steel plants in China have implemented bottom-blowing CO2 technology in converters to achieve CO2 recycling and reduce carbon emissions. The reaction between CO2 and [C] is endothermic, generating 1.2 to 2 times the volume of CO bubbles. This not only lowers the temperature of the molten steel but also enhances the stirring of the molten pool, which is beneficial for improving the dephosphorization rate in the converter.

[0004] In actual production, the converter lining is made of magnesia-carbon bricks, which contain 10-20% carbon. When CO2 is blown into the converter bottom, the CO2 easily reacts with the carbon in the high-temperature magnesia-carbon bricks at the tuyeres, causing erosion of the refractory material at the bottom tuyeres and reducing the life of the converter bottom. The erosion is particularly severe when the converter is blown into the bottom with a high flow rate of CO2.

[0005] In order to ensure the bottom blowing effect, domestic and foreign companies have adopted different countermeasures: (1) sacrifice furnace life to maintain reblowing. European countries have adopted this technology, which has caused the converter furnace life to be taken off the production line at 3000 cycles; (2) adopt the technology of quickly replacing bottom blowing gas supply elements, which has caused the converter to stop and affect production; (3) replace the small furnace bottom when the converter is hot. Replacing the small furnace bottom when the furnace life is 3000 cycles not only affects the production rhythm, but also increases costs. Summary of the Invention

[0006] To address some or all of the technical problems existing in the prior art, the present invention provides a method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2, comprising:

[0007] Bottom blowing assembly design: Multiple bottom blowing assemblies are evenly distributed along the circumference of the converter bottom concentric circles with a diameter of 0.4 to 0.6D, where D is the diameter of the converter bottom. Each bottom blowing assembly is designed to include a central tube and a ring tube. The central tube is concentrically set at the center of the ring tube. The outer wall of the central tube and the inner wall of the ring tube are separated and fixed by a spacer element. The central tube is designed to spray CO2 gas, and the ring tube is designed to spray inert gases such as N2 or Ar.

[0008] Bottom blowing parameter control: The bottom lance performs bottom blowing in the converter through the bottom blowing assembly. The bottom blowing parameters are controlled as follows at different stages of smelting:

[0009] (1) In the early stage of smelting, i.e., within 0 to 5 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. Among them, CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply intensity of the central pipe and the ring pipe is controlled at 0.10 to 0.18 Nm. 3 / (min·t), the bottom blowing gas flow ratio of CO2 injected by the central pipe and N2 injected by the ring pipe is controlled at 4:1;

[0010] (2) During the mid-stage of smelting, specifically within 6–15 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. CO2 is injected through the central pipe, and N2 is injected through the ring pipe. The gas supply intensity of the central and ring pipes is controlled at 0.08–0.16 Nm³. 3 / (min·t), the bottom blowing gas flow ratio of CO2 injected by the central pipe and N2 injected by the ring pipe is controlled at 3:1;

[0011] (3) In the later stage of smelting, i.e., within 16 to 20 minutes of blowing, CO2 + Ar gas is blown from the bottom of the converter. Among them, CO2 is injected through the central pipe and Ar gas is injected through the ring pipe. The gas supply intensity of the central pipe and the ring pipe is controlled at 0.15 to 0.20 Nm. 3 / (min·t), the ratio of the bottom-blown gas flow rate of CO2 injected from the central pipe to Ar gas injected from the ring pipe is controlled at 5:1.

[0012] Furthermore, in the above method for preventing bottom erosion of the converter with high-flow-rate bottom-blown CO2, the flow rates of CO2 gas injected through the central tube and N2 or Ar gas gas injected through the annular tube for each bottom-blown assembly are specifically controlled as follows, based on the ratio of the flow rates of CO2 injected through the central tube to N2 or Ar gas gas injected through the annular tube: the flow rate of bottom-blown gas for each bottom-blown assembly = converter tonnage × gas supply intensity / number of bottom-blown assemblies; the flow rate of CO2 gas injected through the central tube for each bottom-blown assembly = the flow rate of bottom-blown gas for each bottom-blown assembly × the proportion of the flow rate of CO2 gas injected through the central tube; and the flow rate of N2 or Ar gas gas injected through the annular tube for each bottom-blown assembly = the flow rate of bottom-blown gas for each bottom-blown assembly × the proportion of the flow rate of N2 or Ar gas gas injected through the annular tube.

[0013] Furthermore, in the above method for preventing the bottom erosion of the converter by high-flow-rate bottom-blowing CO2, the gas supply pressure of the central tube and the ring tube is controlled at 0.9 MPa during the bottom blowing process of the converter through the bottom blowing assembly.

[0014] Furthermore, in the above-mentioned method for preventing bottom erosion of converters with high-flow-rate bottom-blown CO2, the number of bottom-blowing components is 4 to 12 for converters with a capacity of 80 to 300 tons.

[0015] Furthermore, in the above-mentioned method for preventing the bottom erosion of the converter with high-flow-rate bottom-blown CO2, the bottom-blowing assembly is made of stainless steel.

[0016] As a specific implementation method, the above-mentioned method for preventing bottom erosion of the converter with high-flow-rate bottom-blown CO2 is applied to the steelmaking process of a 180-ton converter. Six bottom-blowing components are evenly distributed along the circumference of a concentric circle with a diameter of 0.6D around the converter bottom. The bottom-blowing parameters are controlled as follows at different stages of smelting:

[0017] (1) In the early stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.13 to 0.18 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.13~0.18Nm 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 4 / 5=(3.12~4.32)Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.13~0.18Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × N2 gas flow rate ratio of ring pipe injection 1 / 5 = (0.78~1.08) Nm 3 / min;

[0018] (2) During the middle stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.10–0.16 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.10~0.16Nm 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 3 / 4 = (2.25~3.6) Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.10~0.16Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × 1 / 4 of the N2 gas flow rate of the annular jet = (0.75~1.2) Nm 3 / min;

[0019] (3) In the later stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.15–0.20 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly and the Ar gas flow rate injected by the ring pipe are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.15~0.20Nm³ / t). 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 5 / 6=(3.75~5.0)Nm 3 / min, and the gas flow rate of Ar gas injected through the annular pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.15~0.20Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × Ar gas flow rate ratio of annular jet injection 1 / 6 = (0.75~1.0) Nm 3 / min.

[0020] As a specific implementation method, the above-mentioned method for preventing bottom erosion of the converter with high-flow-rate bottom-blown CO2 is applied to the steelmaking process of an 80-ton converter. Four bottom-blowing components are evenly distributed along the circumference of a concentric circle with a diameter of 0.5D around the converter bottom. The bottom-blowing parameters are controlled as follows at different stages of smelting:

[0021] (1) In the early stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.10 to 0.15 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.10~0.15Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 4 / 5=(1.6~2.4)Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.10~0.15Nm 3 / (min·t)) / Number of bottom-blowing components 4 × N2 gas flow rate ratio of ring pipe injection 1 / 5 = (0.4~0.6) Nm 3 / min;

[0022] (2) During the middle stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.08–0.14 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.08~0.14Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 3 / 4 = (1.2~2.1) Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.08~0.14Nm³). 3 / (min·t)) / Number of bottom-blowing components 4 × N2 gas flow rate ratio of ring pipe injection 1 / 4 = (0.4~0.7) Nm 3 / min;

[0023] (3) In the later stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.16–0.18 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly and the Ar gas flow rate injected by the ring pipe are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.16~0.18Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 5 / 6=(2.67~3.0)Nm 3 / min, and the gas flow rate of Ar gas injected through the annular pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.16~0.18Nm). 3 / (min·t)) / Number of bottom-blowing components 4 × Ar gas flow rate ratio of annular jet injection 1 / 6 = (0.53~0.6) Nm 3 / min.

[0024] The method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 in this invention has the following advantages and beneficial effects:

[0025] 1. By designing a novel bottom-blowing assembly, CO2 gas is injected through the central pipe, while inert gases such as N2 and Ar are injected through the ring pipe. The ratio of CO2 to inert gas flow rate during different stages of converter smelting is controlled, along with the intensity of bottom-blowing gas supply. This utilizes the inert gas injected through the ring pipe to isolate the CO2 injected through the central pipe from contact with the refractory material at the furnace bottom, preventing the reaction between CO2 and C in the refractory material. This effectively reduces the rate of furnace bottom erosion and allows for the implementation of high-flow-rate bottom-blowing CO2 throughout the process while avoiding furnace bottom erosion. This achieves synchronization between the lifespan of the converter furnace bottom and the overall lifespan of the converter.

[0026] 2. By designing a novel bottom-blowing assembly, CO2 gas is injected through the central pipe, while inert gases such as N2 and Ar are injected through the ring pipe. This dual-layer gas supply creates a clustering effect, allowing the CO2 gas to penetrate deep into the molten steel, promoting the decarburization reaction and generating twice the amount of CO gas. This enhances the stirring effect of the molten pool, thereby increasing the decarburization speed in the converter, shortening the converter smelting time, and simultaneously achieving CO2 recovery and utilization, reducing smelting costs and carbon emissions.

[0027] 3. By bottom blowing CO2 at a high flow rate through the central tube, CO2 participates in the decarburization reaction during the smelting process. Since C + CO2 = 2CO↑ is an endothermic reaction, it can reduce the temperature of the molten pool, promote the dephosphorization reaction, and at the same time reduce the oxidation loss of iron at high temperature, thereby improving the metal yield. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. In the drawings:

[0029] Figure 1 This is a schematic diagram of the bottom blowing assembly designed in the method for preventing bottom erosion of a converter with high flow rate bottom blowing CO2 according to Embodiment 1 of the present invention;

[0030] Figure 2 This is a schematic diagram of the bottom blowing assembly designed in the method for preventing bottom erosion of a converter with high flow rate bottom blowing CO2 according to Embodiment 2 of the present invention;

[0031] Figure 3 This is a schematic diagram of the bottom blowing assembly used in the method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 according to the present invention. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments and corresponding drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0033] The method of the present invention for preventing bottom erosion of converter with high-flow-rate bottom-blown CO2 includes:

[0034] Bottom blowing assembly design: Multiple bottom blowing assemblies are evenly distributed along the circumference of the converter bottom concentric circles with a diameter of 0.4 to 0.6D, where D is the diameter of the converter bottom. Each bottom blowing assembly is designed to include a central tube and a ring tube. The central tube is concentrically set at the center of the ring tube. The outer wall of the central tube and the inner wall of the ring tube are separated and fixed by a spacer element. The central tube is designed to spray CO2 gas, and the ring tube is designed to spray inert gases such as N2 or Ar.

[0035] Bottom blowing parameter control: After the converter tapping is completed and scrap steel and molten iron are added, oxygen blowing with the top lance begins. The bottom lance performs bottom blowing of the converter through the bottom blowing assembly. The bottom blowing parameters are controlled at different stages of smelting as follows:

[0036] (1) In the early stage of smelting, i.e., within 0 to 5 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. Among them, CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.10 to 0.18 Nm. 3 / (min·t), the bottom-blowing gas flow ratio of CO2 injected by the central tube and N2 injected by the ring tube is controlled at 4:1. During this stage, some CO2 gas participates in desiliconization, and the reaction Si + 2CO2 = SiO2 + 2CO↑ occurs, which accelerates the desiliconization rate, generates twice the amount of CO gas, and promotes the stirring of the molten pool;

[0037] (2) During the mid-stage of smelting, specifically within 6–15 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. CO2 is injected through the central pipe, and N2 is injected through the ring pipe. The gas supply pressure for both the central and ring pipes is 0.9 MPa, and the gas supply intensity is 0.08–0.16 Nm³. 3 / (min·t), the bottom-blowing gas flow ratio of CO2 injected through the central pipe to N2 injected through the ring pipe is controlled at 3:1. During this stage, CO2 gas participates in the decarbonization reaction, resulting in the reaction C + CO2 = 2CO↑, accelerating the decarbonization rate, generating twice the amount of CO gas, and promoting molten pool stirring;

[0038] (3) In the later stage of smelting, i.e., within 16 to 20 minutes of blowing, CO2 + Ar gas is blown from the bottom of the converter. CO2 is injected through the central pipe and Ar gas is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.15 to 0.20 Nm. 3 / (min·t), the ratio of CO2 injected through the central pipe to Ar gas injected through the ring pipe is controlled at 5:1. During this stage, due to the low C content in the molten steel, CO2 gas acts as an inert gas to stir the molten steel and basically does not participate in the reaction.

[0039] Furthermore, in the method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 according to the present invention, the flow rate of CO2 gas injected through the central tube and the flow rate of N2 or Ar gas injected through the annular tube for each bottom-blown component are specifically controlled in the following manner according to the ratio of the flow rate of CO2 injected through the central tube to the flow rate of N2 or Ar gas injected through the annular tube: the flow rate of bottom-blown gas for each bottom-blown component = converter tonnage × gas supply intensity / number of bottom-blown components, the flow rate of CO2 gas injected through the central tube for each bottom-blown component = the flow rate of bottom-blown gas for each bottom-blown component × the proportion of the flow rate of CO2 gas injected through the central tube, and the flow rate of N2 or Ar gas injected through the annular tube for each bottom-blown component = the flow rate of bottom-blown gas for each bottom-blown component × the proportion of the flow rate of N2 or Ar gas injected through the annular tube.

[0040] Furthermore, in the method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 according to the present invention, the number of bottom-blowing components can be determined according to the different tonnages of the converter. For example, for an 80-300 ton converter, there can be 4-12 bottom-blowing components; preferably, for an 80-ton converter, there can be 4 bottom-blowing components, and for a 180-ton converter, there can be 6 bottom-blowing components.

[0041] Furthermore, in the method of preventing erosion of the bottom of a converter with high-flow-rate bottom-blown CO2 according to the present invention, the bottom-blowing assembly is preferably made of stainless steel.

[0042] In the method for preventing bottom erosion of converter furnaces by high-flow-rate bottom-blowing CO2 of the present invention, a novel bottom-blowing assembly is designed, in which CO2 gas is injected from the central pipe and inert gases such as N2 and Ar are injected from the ring pipe. This double-layer gas supply creates a clustering effect, allowing the CO2 gas to be injected into the interior of the molten steel, promoting the decarburization reaction and creating twice the gas volume, which enhances the stirring effect of the molten pool. At the same time, the inert gas injected from the ring pipe forms a protective atmosphere around the CO2 injected from the central pipe, isolating the CO2 gas from contact with the furnace bottom refractory material, preventing the reaction between CO2 and C in the refractory material, effectively reducing the furnace bottom erosion rate, and avoiding furnace bottom erosion while achieving high-flow-rate bottom blowing throughout the process.

[0043] The following detailed description of the method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2, in conjunction with specific embodiments, illustrates the present invention.

[0044] Example 1

[0045] Example 1 was applied to a 180-ton converter steelmaking process, such as Figure 1 and 3 As shown, the bottom-blowing assembly is designed as follows: six bottom-blowing assemblies 2 are evenly distributed along the circumference of a concentric circle with a diameter of 0.6D around the converter bottom 1, where D is the diameter of the converter bottom 1. Each bottom-blowing assembly 2 is designed to include a central pipe 21 and a ring pipe 22. The central pipe 21 is concentrically positioned at the center of the ring pipe 22. The outer wall of the central pipe 21 and the inner wall of the ring pipe 22 are separated and fixed by a spacer element 23. The central pipe 21 is designed for blowing CO2 gas, and the ring pipe 22 is designed for blowing inert gases such as N2 or Ar. The bottom-blowing parameters are controlled as follows during different smelting stages:

[0046] (1) In the early stage of smelting, CO2 + N2 gas is blown from the bottom of the converter within 0 to 5 minutes of blowing. CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.13 to 0.18 Nm. 3 / (min·t), the ratio of CO2 injected through the central tube to N2 injected through the ring tube is controlled at 4:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the N2 gas flow rate injected through the ring tube for each bottom blowing assembly are obtained as follows: based on the converter tonnage of 180 tons × gas supply intensity (0.13~0.18Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated to be (3.9~5.4) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (3.9~5.4) Nm 3 / min × CO2 gas flow rate ratio injected through the central pipe: 4 / 5 = (3.12~4.32) Nm 3 / min, and the gas flow rate of N2 injected through the annular pipe of each bottom-blowing assembly = (3.9~5.4) Nm 3 / min × the proportion of N2 gas flow rate in the ring pipe injection is 1 / 5 = (0.78~1.08) Nm 3 / min;

[0047] (2) During the middle stage of smelting, within 6–15 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.10–0.16 Nm. 3 / (min·t), the bottom-blowing gas flow ratio of CO2 injected through the central tube to N2 injected through the ring tube is controlled at 3:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the N2 gas flow rate injected through the ring tube for each bottom-blowing assembly are obtained as follows: based on the converter tonnage of 180 tons × gas supply intensity (0.10~0.16Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated as (3.0~4.8) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (3.0~4.8) Nm 3 / min × CO2 gas flow rate injected through the central pipe accounts for 3 / 4 = (2.25~3.6) Nm 3 / min, and the gas flow rate of N2 injected through the annular pipe of each bottom-blowing assembly = (3.0~4.8) Nm 3 / min × the proportion of N2 gas flow rate in the loop injection is 1 / 4 = (0.75~1.2) Nm 3 / min;

[0048] (3) In the later stage of smelting, i.e., within 16 to 20 minutes of blowing, CO2 + Ar gas is blown from the bottom of the converter. CO2 is injected through the central pipe and Ar gas is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.15 to 0.20 Nm. 3 / (min·t), the ratio of CO2 injected through the central tube to Ar gas injected through the ring tube is controlled at 5:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the Ar gas flow rate injected through the ring tube for each bottom blowing assembly are obtained as follows: based on the converter tonnage of 180 tons × gas supply intensity (0.15~0.20Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated to be (4.5~6.0) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (4.5~6.0) Nm 3 / min × CO2 gas flow rate injected through the central pipe accounts for 5 / 6 = (3.75~5.0) Nm 3 / min, and the Ar gas flow rate injected through the annular pipe of each bottom-blowing assembly = (4.5~6.0) Nm 3 / min × Ar gas flow rate ratio of the ring pipe injection 1 / 6 = (0.75~1.0) Nm 3 / min.

[0049] Actual calculations show that, using Embodiment 1 of this invention, the 180t converter achieves full-process high-flow-rate bottom-blown CO2 gas smelting, effectively avoiding the erosion of the furnace bottom refractory material, and the converter bottom life reaches 8200 heats, achieving synchronization with the converter furnace life.

[0050] Example 2

[0051] Example 2 was applied to an 80-ton converter steelmaking process, such as Figure 2 and 3 As shown, the bottom-blowing assembly is designed as follows: four bottom-blowing assemblies 2' are evenly distributed along the circumference of a concentric circle with a diameter of 0.5D around the converter bottom 1', where D is the diameter of the converter bottom 1'. Each bottom-blowing assembly 2' is designed to include a central pipe 21 and a ring pipe 22. The central pipe 21 is concentrically positioned at the center of the ring pipe 22. The outer wall of the central pipe 21 and the inner wall of the ring pipe 22 are separated and fixed by a spacer element 23. The central pipe 21 is designed for blowing CO2 gas, and the ring pipe 22 is designed for blowing inert gases such as N2 or Ar. The bottom-blowing parameters are controlled as follows at different stages of smelting:

[0052] (1) In the early stage of smelting, CO2 + N2 gas is blown from the bottom of the converter within 0 to 5 minutes of blowing. Among them, CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.10 to 0.15 Nm. 3 / (min·t), the bottom-blowing gas flow ratio of CO2 injected through the central tube to N2 injected through the ring tube is controlled at 4:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the N2 gas flow rate injected through the ring tube for each bottom-blowing assembly are obtained as follows: based on the converter tonnage of 80 tons × gas supply intensity (0.10~0.15Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated as (2.0~3.0) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (2.0~3.0) Nm 3 / min × CO2 gas flow rate injected through the central pipe accounts for 4 / 5 = (1.6~2.4) Nm 3 / min, and the gas flow rate of N2 injected through the annular pipe of each bottom-blowing assembly = (2.0~3.0) Nm 3 / min × the proportion of N2 gas flow rate in the loop injection is 1 / 5 = (0.4~0.6) Nm 3 / min;

[0053] (2) During the mid-stage of smelting, within 6–15 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. CO2 is injected through the central pipe, and N2 is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.08–0.14 Nm. 3 / (min·t), the ratio of CO2 injected through the central tube to N2 injected through the ring tube is controlled at 3:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the N2 gas flow rate injected through the ring tube for each bottom blowing assembly are obtained as follows: based on the converter tonnage of 80 tons × gas supply intensity (0.08~0.14Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated as (1.6~2.8) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (1.6~2.8) Nm 3 / min × CO2 gas flow rate injected through the central pipe accounts for 3 / 4 = (1.2~2.1) Nm 3 / min, and the gas flow rate of N2 injected through the annular pipe of each bottom-blowing assembly = (1.6~2.8) Nm 3 / min × the proportion of N2 gas flow rate in the loop injection is 1 / 4 = (0.4~0.7) Nm 3 / min;

[0054] (3) In the later stage of smelting, i.e., within 16 to 20 minutes of blowing, CO2 + Ar gas is blown from the bottom of the converter. CO2 is injected through the central pipe and Ar gas is injected through the ring pipe. The gas supply pressure of the central pipe and the ring pipe is 0.9 MPa and the gas supply intensity is 0.16 to 0.18 Nm. 3 / (min·t), the ratio of CO2 injected through the central tube to Ar gas injected through the ring tube is controlled at 5:1, and the specific values ​​of the CO2 gas flow rate injected through the central tube and the Ar gas flow rate injected through the ring tube for each bottom blowing assembly are obtained as follows: based on the converter tonnage of 80 tons × gas supply intensity (0.16~0.18Nm). 3 The bottom-blowing gas flow rate for each bottom-blowing component is calculated as (3.2~3.6) Nm³ / (min·t) / number of bottom-blowing components. 3 / min, therefore the CO2 gas flow rate injected by the central pipe of each bottom blowing assembly = (3.2~3.6) Nm 3 / min × CO2 gas flow rate injected through the central pipe accounts for 5 / 6 = (2.67~3.0) Nm 3 / min, and the gas flow rate of Ar gas injected through the annular pipe of each bottom-blowing assembly = (3.2~3.6) Nm 3 / min × Ar gas flow rate ratio of the ring pipe injection 1 / 6 = (0.53~0.6) Nm3 / min.

[0055] Actual calculations show that, using Embodiment 2 of this invention, the 80t converter achieves full-process high-flow-rate bottom-blown CO2 gas smelting, effectively avoiding the erosion of the furnace bottom refractory material, and the converter bottom life reaches 7800 heats, achieving synchronization with the converter furnace life.

[0056] In summary, compared with the prior art, the method of the present invention for preventing bottom erosion of converters with high-flow-rate bottom-blown CO2 has the following advantages and beneficial effects:

[0057] By designing a novel bottom-blowing assembly, CO2 gas is injected through a central tube, while inert gases such as N2 and Ar are injected through a ring tube. The ratio of CO2 to inert gas flow rates during different stages of converter smelting is controlled, along with the intensity of bottom-blowing gas supply. This utilizes the inert gas injected through the ring tube to isolate the CO2 injected through the central tube from contact with the refractory material at the furnace bottom, preventing the reaction between CO2 and C in the refractory material. This effectively reduces the rate of furnace bottom erosion, achieving high-flow-rate bottom-blowing of CO2 throughout the process while avoiding furnace bottom erosion. This synchronizes the lifespan of the converter furnace bottom with the age of the converter.

[0058] By designing a novel bottom-blowing assembly, CO2 gas is injected through a central pipe, while inert gases such as N2 and Ar are injected through ring pipes. This dual-layer gas supply creates a clustering effect, allowing the CO2 gas to be injected into the molten steel, promoting the decarburization reaction and generating twice the amount of CO gas, thus enhancing the stirring effect of the molten pool. This increases the decarburization speed in the converter, shortens the converter smelting time, and simultaneously achieves CO2 recovery and utilization, reducing smelting costs and carbon emissions.

[0059] By bottom-blowing CO2 at a high flow rate through the central tube, CO2 participates in the decarburization reaction during the smelting process. Since C + CO2 = 2CO↑ is an endothermic reaction, it can reduce the temperature of the molten pool, promote the dephosphorization reaction, and at the same time reduce the oxidation loss of iron at high temperatures, thereby improving the metal yield.

[0060] It should be noted that, in this document, the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preventing erosion of the furnace bottom in a converter using high-flow-rate bottom-blown CO2, characterized in that, include: Bottom blowing assembly design: Multiple bottom blowing assemblies are evenly distributed along the circumference of the converter bottom concentric circles with a diameter of 0.4 to 0.6D, where D is the diameter of the converter bottom. Each bottom blowing assembly is designed to include a central tube and a ring tube. The central tube is concentrically set at the center of the ring tube. The outer wall of the central tube and the inner wall of the ring tube are separated and fixed by a spacer element. The central tube is designed to spray CO2 gas, and the ring tube is designed to spray N2 or Ar. Bottom blowing parameter control: The bottom lance performs bottom blowing in the converter through the bottom blowing assembly. The bottom blowing parameters are controlled as follows at different stages of smelting: (1) In the early stage of smelting, i.e., within 0 to 5 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. Among them, CO2 is injected through the central pipe and N2 is injected through the ring pipe. The gas supply intensity of the central pipe and the ring pipe is controlled at 0.10 to 0.18 Nm. 3 / (min·t), the bottom blowing gas flow ratio of CO2 injected by the central pipe and N2 injected by the ring pipe is controlled at 4:1; (2) During the mid-stage of smelting, specifically within 6–15 minutes of blowing, CO2 + N2 gas is blown from the bottom of the converter. CO2 is injected through the central pipe, and N2 is injected through the ring pipe. The gas supply intensity of the central and ring pipes is controlled at 0.08–0.16 Nm³. 3 / (min·t), the bottom blowing gas flow ratio of CO2 injected by the central pipe and N2 injected by the ring pipe is controlled at 3:1; (3) In the later stage of smelting, i.e., within 16 to 20 minutes of blowing, CO2 + Ar gas is blown from the bottom of the converter. Among them, CO2 is injected through the central pipe and Ar gas is injected through the ring pipe. The gas supply intensity of the central pipe and the ring pipe is controlled at 0.15 to 0.20 Nm. 3 / (min·t), the ratio of the bottom-blown gas flow rate of CO2 injected from the central pipe to Ar gas injected from the ring pipe is controlled at 5:

1.

2. The method for preventing erosion of the converter bottom by high-flow-rate bottom-blown CO2 as described in claim 1, characterized in that, Based on the ratio of CO2 injected through the central tube to N2 or Ar injected through the ring tube, the CO2 gas flow rate injected through the central tube and the N2 or Ar gas flow rate injected through the ring tube for each bottom blowing assembly are specifically controlled as follows: Bottom blowing gas flow rate for each bottom blowing assembly = converter tonnage × gas supply intensity / number of bottom blowing assemblies; CO2 gas flow rate injected through the central tube for each bottom blowing assembly = bottom blowing gas flow rate for each bottom blowing assembly × percentage of CO2 gas flow rate injected through the central tube; and N2 or Ar gas flow rate injected through the ring tube for each bottom blowing assembly = bottom blowing gas flow rate for each bottom blowing assembly × percentage of N2 or Ar gas flow rate injected through the ring tube.

3. The method for preventing erosion of the converter bottom by high-flow-rate bottom-blown CO2 as described in claim 1, characterized in that, During the bottom blowing process of the converter through the bottom blowing assembly, the gas supply pressure of the central tube and the ring tube is controlled at 0.9 MPa.

4. The method for preventing erosion of the converter bottom by high-flow-rate bottom-blown CO2 as described in claim 1, characterized in that, For converters with a capacity of 80 to 300 tons, the number of bottom-blowing components is 4 to 12.

5. The method for preventing erosion of the converter bottom by high-flow-rate bottom-blown CO2 as described in claim 1, characterized in that, The bottom blowing component is made of stainless steel.

6. The method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 as described in claim 1, applied to a 180-ton converter steelmaking process, is characterized in that... Six bottom-blowing components are evenly distributed along the circumference of a concentric circle with a diameter of 0.6D at the bottom of the converter. The bottom-blowing parameters are controlled as follows at different stages of smelting: (1) In the early stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.13 to 0.18 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.13~0.18Nm 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 4 / 5=(3.12~4.32)Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.13~0.18Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × N2 gas flow rate ratio of ring pipe injection 1 / 5 = (0.78~1.08) Nm 3 / min; (2) During the middle stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.10–0.16 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.10~0.16Nm 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 3 / 4 = (2.25~3.6) Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.10~0.16Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × 1 / 4 of the N2 gas flow rate of the annular jet = (0.75~1.2) Nm 3 / min; (3) In the later stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.15–0.20 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly and the Ar gas flow rate injected by the ring pipe are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.15~0.20Nm³ / t). 3 / (min·t)) / Number of bottom-blowing components 6 × CO2 gas flow rate ratio of central tube injection 5 / 6=(3.75~5.0)Nm 3 / min, and the gas flow rate of Ar gas injected through the annular pipe of each bottom-blowing assembly = converter tonnage 180 tons × gas supply intensity (0.15~0.20Nm³). 3 / (min·t)) / Number of bottom-blowing components 6 × Ar gas flow rate ratio of annular jet injection 1 / 6 = (0.75~1.0) Nm 3 / min.

7. The method for preventing bottom erosion of a converter with high-flow-rate bottom-blown CO2 as described in claim 1, applied to an 80-ton converter steelmaking process, is characterized in that... Four bottom-blowing components are evenly distributed along the circumference of a concentric circle with a diameter of 0.5D at the bottom of the converter. The bottom-blowing parameters are controlled as follows at different stages of smelting: (1) In the early stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.10 to 0.15 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.10~0.15Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 4 / 5=(1.6~2.4)Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.10~0.15Nm 3 / (min·t)) / Number of bottom-blowing components 4 × N2 gas flow rate ratio of ring pipe injection 1 / 5 = (0.4~0.6) Nm 3 / min; (2) During the middle stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.08–0.14 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe and the N2 gas flow rate injected by the ring pipe of each bottom-blowing assembly are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.08~0.14Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 3 / 4 = (1.2~2.1) Nm 3 / min, and the N2 gas flow rate of the annular injection of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.08~0.14Nm³). 3 / (min·t)) / Number of bottom-blowing components 4 × N2 gas flow rate ratio of ring pipe injection 1 / 4 = (0.4~0.7) Nm 3 / min; (3) In the later stage of smelting, the gas supply pressure of the central pipe and the ring pipe is 0.9 MPa, and the gas supply intensity is 0.16–0.18 Nm. 3 / (min·t), the specific values ​​of the CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly and the Ar gas flow rate injected by the ring pipe are controlled as follows: CO2 gas flow rate injected by the central pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.16~0.18Nm 3 / (min·t)) / Number of bottom-blowing components 4 × CO2 gas flow rate ratio of central tube injection 5 / 6=(2.67~3.0)Nm 3 / min, and the gas flow rate of Ar gas injected through the annular pipe of each bottom-blowing assembly = converter tonnage 80 tons × gas supply intensity (0.16~0.18Nm). 3 / (min·t)) / Number of bottom-blowing components 4 × Ar gas flow rate ratio of annular jet injection 1 / 6 = (0.53~0.6) Nm 3 / min.

Citation Information

Patent Citations

  • Steel-making method for prolonging service life of bottom-blowing oxygen converter through CO2

    CN105907914A

  • Bottom spraying type limestone smelting method of combined top-bottom combined blowing converter

    CN109852762A